Battery and method for manufacturing electrode
By using Bi and Mn alloys as active material layers for electrodes in lithium secondary batteries, the problem of poor cycle characteristics caused by electrode expansion and contraction is solved through electroplating and heat treatment technology, and the battery performance with high energy efficiency and long cycle life is achieved .
Patent Information
- Application Number
- CN202380018101.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-25
- Filing Date
- 2023-01-11
- Publication Date
- 2024-11-08
AI Technical Summary
In existing lithium secondary batteries, the expansion and contraction of electrode active substances lead to poor circulation characteristics, and the traditional electroplating process is high and the manufacturing cost is not practical, making it difficult to achieve high energy efficiency and long cycle life.
An alloy containing Bi and Mn is used as an active material layer of the electrode, and an alloy thin film such as BiMn or Bi4Mn3Cu4 is formed on the current collector by electroplating, and heat treatment is performed to form an active material layer with high density and good electron conduction pathways.
The energy efficiency and circulation characteristics of lithium secondary batteries are improved, the impact of expansion and contraction of electrodes on current collecting characteristics is reduced, and the battery performance with high capacity and long cycle life is achieved.
Smart Images

Figure CN118922958A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to methods of making batteries and electrodes. Background Art
[0002] In recent years, research and development of lithium secondary batteries has been actively carried out. The battery characteristics such as charge and discharge voltage, charge and discharge cycle life characteristics, and storage characteristics are greatly affected by the electrodes used. Therefore, the battery characteristics can be improved by improving the electrode active material.
[0003] For example, lithium secondary batteries using aluminum, silicon, tin, etc., which are electrochemically alloyed with lithium during charging, as electrodes have been proposed. Patent document 1 discloses a lithium secondary battery having a negative electrode including a negative electrode material formed of an alloy having silicon, tin and a transition metal, a positive electrode, and an electrolyte.
[0004] Patent Document 2 discloses a lithium secondary battery including a negative electrode using a silicon thin film provided on a current collector as an active material, a positive electrode, and an electrolyte.
[0005] Examples of metals that alloy with lithium include bismuth (Bi). Non-Patent Document 1 discloses a negative electrode made of Bi powder and containing Bi as a negative electrode active material.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 4898737
[0009] Patent Document 2: Japanese Patent No. 3733065
[0010] Non-patent literature
[0011] Non-patent document 1: Hiroyuki Yamaguchi, "Synthesis and electrochemical properties of amorphous polymer negative electrode active materials for lithium batteries formed from the reaction products of polyacrylic acid and metal oxides," Mie University, PhD thesis, 2015 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] The present disclosure provides batteries with improved energy efficiency.
[0014] Solutions for solving problems
[0015] The battery disclosed herein has:
[0016] The first electrode,
[0017] the second electrode, and
[0018] an electrolyte layer located between the first electrode and the second electrode,
[0019] The first electrode has:
[0020] Current collector, and
[0021] an active material layer located between the current collector and the electrolyte layer,
[0022] The active material layer contains an alloy containing Bi and Mn.
[0023] Effects of the Invention
[0024] According to the present disclosure, a battery having improved energy efficiency can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a cross-sectional view schematically showing a configuration example of a battery according to an embodiment of the present disclosure.
[0026] Figure 2 It is a cross-sectional view schematically showing a modification of the battery according to the embodiment of the present disclosure.
[0027] Figure 3 The graphs show X-ray diffraction patterns of the active material layer of the first electrode in the battery of Example 1 at the initial stage, after charge, and after charge and discharge.
[0028] Figure 4 3 is a graph showing the results of a charge and discharge test of the battery of Example 1.
[0029] Figure 5 This is a graph showing the results of a charge and discharge test of the battery of Example 2.
[0030] Figure 6 Graphs showing the results of a charge and discharge test of the battery of Example 3.
[0031] Figure 7 The graphs show X-ray diffraction patterns of the active material layer of the first electrode in the battery of Example 4 at the initial stage, after charge, and after charge and discharge.
[0032] Figure 8 Graphs showing the results of a charge and discharge test of the battery of Example 4.
[0033] Fig. 9 Graphs showing the results of a charge and discharge test of the battery of Example 5.
[0034] Fig.10 This is a graph showing the results of a charge and discharge test of the battery of Example 6.
[0035] Fig.113 is a graph showing the results of a charge and discharge test of the battery of Reference Example 1.
[0036] Fig.12 3 is a graph showing the results of a charge and discharge test of the battery of Reference Example 2.
[0037] Fig.13 Graphs showing the results of a charge and discharge test of the battery of Reference Example 3. DETAILED DESCRIPTION
[0038] (Insights that form the basis of this disclosure)
[0039] As described in the column of “Background Art”, in lithium secondary batteries, improvements in battery characteristics are achieved by improving electrode active materials.
[0040] When lithium metal is used as the negative electrode active material, a lithium secondary battery with high energy density per unit weight and per unit volume is obtained. However, in a lithium secondary battery with such a structure, lithium is precipitated in a dendritic shape during charging. A portion of the precipitated lithium metal reacts with the electrolyte, so there is a problem of low charge and discharge efficiency and poor cycle characteristics.
[0041] In contrast, it is proposed to use carbon, especially graphite, as a negative electrode. In the negative electrode using carbon, charging and discharging are performed by embedding and de-embedding lithium into carbon. In the negative electrode having such a structure, lithium metal does not precipitate in a dendritic shape in the charge and discharge mechanism. In addition, in the lithium secondary battery using the negative electrode having such a structure, the reaction is topological, so the reversibility is very good, and the charge and discharge efficiency is basically 100%. As a result, lithium secondary batteries using negative electrodes using carbon, especially graphite, have been put into practical use. However, the theoretical capacity density of graphite is 372mAh / g, which is about 1 / 10 of the theoretical capacity density of lithium metal 3884mAh / g. Therefore, the active material capacity density of the negative electrode using graphite is low. Furthermore, the actual capacity density of graphite basically reaches the theoretical capacity density, so there is a limit to the high capacity in the negative electrode using graphite.
[0042] In contrast, lithium secondary batteries using aluminum, silicon, tin, etc., which are electrochemically alloyed with lithium during charging, as electrodes have been proposed. The capacity density of metals alloyed with lithium is significantly greater than that of graphite. In particular, the theoretical capacity density of silicon is large. Therefore, it is desirable to use electrodes such as aluminum, silicon, tin, etc. alloyed with lithium as negative electrodes for batteries showing high capacity, and various secondary batteries using them as negative electrodes have been proposed (Patent Document 1).
[0043] However, the negative electrode using the metal alloyed with lithium as described above will expand if it absorbs lithium and shrink if it releases lithium. If this expansion and shrinkage are repeated during charge and discharge, the alloy itself, which is the electrode active material, will be pulverized due to charge and discharge, which will deteriorate the current collection characteristics of the negative electrode, and therefore, sufficient cycle characteristics cannot be obtained. In order to improve this shortcoming, the following attempts have been made. For example, an attempt has been made to deposit silicon on a rough surface collector by sputtering or evaporation, or to deposit tin on a rough surface collector by electroplating (Patent Document 2). In this attempt, the active material, that is, the metal alloyed with lithium, becomes a thin film and is in close contact with the collector. Therefore, even if the negative electrode repeatedly expands and shrinks due to the absorption and release of lithium, the current collection property will hardly decrease.
[0044] However, as mentioned above, when the active material is formed by sputtering or evaporation, the manufacturing cost is high and it is not practical. It is practical to form the active material by electroplating, which is cheap in manufacturing cost, but electroplating of silicon is very difficult. In addition, there are problems such as the lack of discharge flatness and difficulty in using it as a battery electrode for tin, which is cheap in electroplating.
[0045] In addition, as a metal alloyed with lithium, bismuth (Bi) can be cited. Bi forms compounds such as LiBi and Li3Bi with lithium (Li). The potential of LiBi and the potential of Li3Bi are almost the same. On the other hand, in the case of tin, which lacks discharge flatness, there are many compounds formed with lithium, and the potentials of each compound are completely different from each other. That is, Bi does not have the property of greatly different potentials between various compounds formed with lithium like tin. Therefore, the potential of the electrode containing Bi as an active material is flat, and therefore, the discharge flatness is excellent. Therefore, it is believed that the electrode containing Bi as an active material is suitable as a battery electrode.
[0046] However, Bi lacks ductility and is difficult to manufacture in the form of metal plates or metal foils, and the resulting form becomes a small ball or powder. Therefore, as an electrode containing Bi as an active material, an electrode manufactured by applying Bi powder to a collector has been studied. However, the electrode manufactured using this Bi powder is micronized by repeated charge and discharge, and the current collection characteristics deteriorate, so that sufficient cycle characteristics cannot be obtained. For example, in non-patent document 1, Bi powder is used and PVdF (polyvinylidene fluoride) or PI (polyimide) is used as a binder to make an electrode containing Bi as an active material. In non-patent document 1, the battery made using the electrode is charged and discharged. However, the initial charge and discharge curves and cycle characteristics of the produced electrode are very poor. It is measured at a very low rate equivalent to 0.042IT, but the initial charge and discharge efficiency is low, and the cycle degradation is also strong, so it is not provided for practical use. Regarding this cycle degradation, Non-Patent Document 1 shows that it is considered that as the Bi active material expands when Li is inserted and shrinks when Li is released, the active material becomes finer and cannot form an electron conduction path, resulting in a decrease in capacity.
[0047] As mentioned above, the inventors of the present invention have focused on Bi, which has excellent discharge flatness and does not have the property of greatly different potentials between various compounds formed with Li, and have conducted intensive research on batteries that can improve cycle characteristics. As a result, the inventors of the present invention have come up with the following new technical concept: using an alloy containing Bi and Mn as an active material.
[0048] (Overview of one aspect of the present disclosure)
[0049] A battery according to a first aspect of the present disclosure includes:
[0050] The first electrode,
[0051] the second electrode, and
[0052] a solid electrolyte layer located between the first electrode and the second electrode,
[0053] The first electrode has:
[0054] Current collector, and
[0055] an active material layer located between the current collector and the electrolyte layer,
[0056] The active material layer contains an alloy containing Bi and Mn.
[0057] The battery of the first embodiment can improve energy efficiency by including an electrode having an active material layer containing an alloy containing Bi and Mn.
[0058] In the second aspect of the present disclosure, for example, in the battery of the first aspect, the active material layer may include at least one selected from the group consisting of LiBi and Li3Bi.
[0059] The battery of the second embodiment can further improve energy efficiency.
[0060] In a third aspect of the present disclosure, for example, in the battery of the first or second aspect, the active material layer may contain BiMn as the active material.
[0061] The battery of the third embodiment can further improve energy efficiency.
[0062] In a fourth aspect of the present disclosure, for example, in the battery of the third aspect, the BiMn may have a crystal structure belonging to a space group of P63 / mmc.
[0063] The battery of the fourth embodiment can further improve energy efficiency.
[0064] In a fifth aspect of the present disclosure, for example, in the battery of any one of the first to fourth aspects, the active material layer may contain Bi4Cu4Mn3 as the active material.
[0065] The battery of the fifth embodiment can further improve energy efficiency.
[0066] In the sixth aspect of the present disclosure, for example, in the battery of the fifth aspect, the Bi4Cu4Mn3 may have a crystal structure whose space group belongs to Fm-3m.
[0067] The battery of the sixth embodiment can further improve energy efficiency.
[0068] In a seventh aspect of the present disclosure, for example, in the battery of any one of the first to sixth aspects, the active material layer may not contain a solid electrolyte.
[0069] The active material layer of the battery of the seventh aspect does not contain a solid electrolyte, so the capacity per unit volume can be increased. Therefore, according to the seventh aspect, a battery having a high capacity per unit volume and improved energy efficiency can be provided.
[0070] In an eighth aspect of the present disclosure, for example, in the battery according to any one of the first to seventh aspects, the current collector may contain Cu.
[0071] In the battery of the eighth embodiment, since the current collector includes Cu, for example, the current collector is used as a substrate, a Bi-plated film and a Mn-plated film are formed on the substrate, and a heat treatment is performed, thereby making it easy to produce an active material layer 104 containing an alloy containing Bi, Mn, and Cu such as Bi4Mn3Cu4. Therefore, according to the eighth embodiment, a battery having a structure suitable for improving energy efficiency can be easily provided.
[0072] In a ninth aspect of the present disclosure, for example, in the battery of any one of the first to eighth aspects, the active material layer may be a heat-treated plating layer.
[0073] The active material layer of the battery of the ninth aspect is a heat-treated plating layer, so the capacity per unit volume can be increased. Therefore, according to the ninth aspect, a battery having a high capacity per unit volume and improved energy efficiency can be provided.
[0074] In a tenth aspect of the present disclosure, for example, in the battery according to any one of the first to ninth aspects, the electrolyte layer may contain an electrolytic solution.
[0075] The battery of the tenth embodiment has improved energy efficiency and good cycle characteristics.
[0076] In the 11th aspect of the present disclosure, for example, in the battery according to the 10th aspect, the electrolyte solution may contain vinylene carbonate as a solvent.
[0077] The battery of the eleventh embodiment has improved energy efficiency and good cycle characteristics.
[0078] In a twelfth aspect of the present disclosure, for example, in the battery of any one of the first to ninth aspects, the electrolyte layer may be a solid electrolyte layer.
[0079] The battery of the twelfth embodiment has improved energy efficiency and good cycle characteristics.
[0080] In the 13th aspect of the present disclosure, for example, in the battery of the 12th aspect, the solid electrolyte layer may include a halide solid electrolyte, and the halide solid electrolyte may not contain sulfur.
[0081] The battery of the thirteenth aspect has improved energy efficiency and good cycle characteristics.
[0082] In a fourteenth aspect of the present disclosure, for example, in the battery according to the twelfth aspect, the solid electrolyte layer may include a sulfide solid electrolyte.
[0083] The battery of the fourteenth aspect has improved energy efficiency and can also have good cycle characteristics.
[0084] In a fifteenth aspect of the present disclosure, for example, in the battery of any one of the first to fourteenth aspects, the first electrode may be a negative electrode, and the second electrode may be a positive electrode.
[0085] The battery of the fifteenth aspect has improved energy efficiency.
[0086] The method for manufacturing an electrode according to the 16th aspect of the present disclosure includes the following steps:
[0087] The step of forming a coating layer including a Bi coating film and a Mn coating film on a current collector by electroplating; and,
[0088] The step of heating the current collector and the plated layer to obtain an electrode having an active material layer formed on the current collector, wherein the active material layer contains an alloy containing Bi and Mn.
[0089] According to the production method of the sixteenth aspect, an electrode capable of improving the energy efficiency of a battery can be easily produced.
[0090] In a seventeenth aspect of the present disclosure, for example, in the production method according to the sixteenth aspect, the current collector may contain Cu.
[0091] According to the manufacturing method of the seventeenth aspect, an electrode capable of improving the energy efficiency of a battery can be easily manufactured.
[0092] (Embodiments of the present disclosure)
[0093] Hereinafter, the embodiments of the present disclosure will be described with reference to the accompanying drawings. The following descriptions all show inclusive examples or specific examples. The numerical values, compositions, shapes, film thicknesses, electrical characteristics, and structures of secondary batteries shown below are examples and are not intended to limit the subject matter of the present disclosure.
[0094] Figure 1 It is a cross-sectional view schematically showing a configuration example of a battery 1000 according to an embodiment of the present disclosure.
[0095] The battery 1000 includes a first electrode 101, a second electrode 103, and an electrolyte layer 102 located between the first electrode 101 and the second electrode 103. The first electrode 101 includes a current collector 100 and an active material layer 104 located between the current collector 100 and the electrolyte layer 102. The active material layer 104 includes an alloy containing Bi and Mn.
[0096] The battery 1000 includes a first electrode 101, which includes an active material layer 104 containing an alloy containing Bi and Mn as an active material. With this structure, the battery 1000 can improve energy efficiency. Here, the energy efficiency of the battery specifically refers to the value calculated by "discharge power (Wh) × 100 / charge power (Wh)". It should be noted that in the evaluation of the energy efficiency of a half-battery unit, that is, a single electrode evaluation, in this specification, a small potential difference (ΔV) between the charge reaction potential and the discharge reaction potential is regarded as high energy efficiency. The potential difference between the charge reaction potential and the discharge reaction potential is evaluated by the potential of the flat part of the charge reaction potential and the potential of the flat part of the discharge reaction potential.
[0097] like Figure 1 As shown, the second electrode 103 includes a current collector 105 and an active material layer 106 .
[0098] In the battery 1000, the electrolyte layer 102 is a solid electrolyte layer. Therefore, even if the active material layer 104 containing an alloy containing Bi and Mn as an active material is repeatedly expanded and contracted according to charge and discharge, the electrolyte containing the electrolyte is not mixed into the active material layer 104. Therefore, the reduction of the electron conduction path in the active material layer 104 based on repeated charge and discharge is suppressed. Therefore, the battery 1000 is not easy to produce a decrease in the current collection property of the active material layer 104 based on charge and discharge, and therefore, it can have good cycle characteristics.
[0099] The battery 1000 is, for example, a lithium secondary battery. Hereinafter, the case where the metal ions absorbed and released by the active material layer 106 of the first electrode 101 and the second electrode 103 during charge and discharge of the battery 1000 is lithium ions will be described as an example.
[0100] As described above, the active material layer 104 contains an alloy containing Bi and Mn. The alloy containing Bi and Mn may be, for example, an intermetallic compound.
[0101] The alloy containing Bi and Mn may be, for example, BiMn. That is, the active material layer 104 may contain BiMn as an active material.
[0102] According to the above configuration, the energy efficiency of the battery 1000 can be further improved.
[0103] BiMn contained in the active material layer 104 may have a crystal structure belonging to a space group of P63 / mmc.
[0104] The alloy containing Bi and Mn may be, for example, Bi4Cu4Mn3. That is, the active material layer 104 may contain Bi4Cu4Mn3 as an active material.
[0105] According to the above configuration, the energy efficiency of the battery 1000 can be further improved.
[0106] Bi 4 Cu 4 Mn 3 contained in the active material layer 104 may have a crystal structure belonging to the space group Fm-3m.
[0107] According to the above configuration, the energy efficiency of the battery 1000 can be further improved.
[0108] The active material layer 104 may contain an alloy containing Bi and Mn as main components. Here, "the active material layer 104 contains an alloy containing Bi and Mn as main components" is defined as "the content ratio of the alloy containing Bi and Mn in the active material layer 104 is 0% by mass or more". It should be noted that the content ratio of the alloy containing Bi and Mn in the active material layer 104 can be calculated, for example, as follows: according to the elemental analysis based on EDX (energy dispersive X-ray analysis), it is confirmed that Bi and Mn are contained in the active material layer 104, and the X-ray diffraction results of the active material layer 104 are subjected to Rietveld analysis to calculate the ratio of the contained compounds (that is, compounds containing Bi and Mn as constituent elements), thereby being able to be calculated. The above-mentioned "compounds containing Bi and Mn as constituent elements" are, for example, BiMn and Bi4Cu4Mn3. When the active material layer 104 contains a plurality of compounds as the alloy containing Bi and Mn, the total of the content ratios of these compounds is the content ratio of the alloy containing Bi and Mn in the active material layer 104 .
[0109] According to the above configuration, the energy efficiency of the battery 1000 can be further improved.
[0110] The active material layer 104 containing an alloy containing Bi and Mn may be composed of, for example, an alloy containing Bi and Mn formed into a thin film (hereinafter referred to as "alloy thin film containing Bi and Mn"). The alloy containing Bi and Mn formed into a thin film may be, for example, BiMn or Bi4Mn3Cu4 formed into a thin film.
[0111] According to the above configuration, the energy efficiency of the battery 1000 can be further improved.
[0112] The active material layer 104 containing an alloy containing Bi and Mn can be produced by, for example, electroplating. The method of producing the active material layer 104 by electroplating to manufacture the first electrode 101 is as follows, for example.
[0113] First, a substrate for electroplating is prepared. In the first electrode 101, for example, the current collector 100 is called the substrate. As the current collector 100, for example, a current collector containing Cu is prepared. The manufacturing method of the first electrode 101, for example, includes the following steps:
[0114] The step of forming a coating layer including a Bi coating film and a Mn coating film on a current collector by electroplating; and,
[0115] The step of heating the current collector and the plated layer to obtain an electrode having an active material layer formed on the current collector, wherein the active material layer contains an alloy containing Bi and Mn.
[0116] The above-mentioned coating layer can be produced by, for example, first forming a Bi coating film and then forming a Mn coating film thereon. The order of producing the Bi coating film and the Mn coating film is not limited thereto, for example, the above-mentioned coating layer can also be produced by first forming a Mn coating film and then forming a Bi coating film thereon.
[0117] In the above manufacturing method, the current collector and the plated layer are heated, so that, for example, Mn in the Mn-plated film, or Mn in the Mn-plated film and Cu contained in the current collector are diffused into the Bi-plated film. Thus, an active material layer containing an alloy containing Bi and Mn, such as BiMn or Bi4Mn3Cu4, can be formed on the current collector.
[0118] The heating temperature of the plating layer may be, for example, 150° C. or higher and 400° C. or lower.
[0119] The method for manufacturing the first electrode 101 will be described in more detail.
[0120] First, prepare a substrate for electroplating. In the first electrode 101, for example, the current collector 1100 becomes the substrate. As an example, prepare copper foil as the current collector 100. After pre-degreasing the copper foil with an organic solvent, mask one side and immerse it in an acidic solvent to degrease and activate the surface of the copper foil. Connect the activated copper foil to a power source in a manner that allows current to be applied. Immerse the copper foil connected to the power source in a bismuth plating bath. As the bismuth plating bath, for example, a bismuth-containing 3+ ions and an organic acid bath of an organic acid. Afterwards, the current density and the application time are controlled to apply current to the copper foil, thereby electroplating Bi on the unmasked surface of the copper foil. After electroplating, the copper foil is recovered from the plating bath, and after removing the mask, it is cleaned and dried with pure water. According to these methods, a Bi-plated film is made on the surface of the copper foil. It should be noted that the bismuth-plating bath used in the preparation of the Bi-plated film is not particularly limited, and can be appropriately selected from the known bismuth-plating baths that can precipitate Bi single-substance thin films. In the bismuth-plating bath, as an organic acid bath, an organic sulfonic acid bath, a gluconic acid and ethylenediaminetetraacetic acid (EDTA) bath, or a citric acid and EDTA bath can be used. In addition, in the bismuth-plating bath, for example, a sulfuric acid bath can also be used. In addition, additives can also be added to the bismuth-plating bath.
[0121] Next, the surface without Bi-plating film is masked again, and the copper foil with Bi-plating film is connected to a power source so that current can be applied. The copper foil connected to the power source is immersed in a manganese plating bath. As the manganese plating bath, for example, a 2+ions and sulfuric acid. Thereafter, the current density and the application time are controlled to apply current to the copper foil, thereby electroplating Mn on the surface of the unmasked Bi-plated film. After electroplating, the Mn-plated copper foil is recovered from the plating bath, and after the mask is removed, it is cleaned and dried with pure water. According to these methods, a Mn-plated film is produced on the Bi-plated film of the copper foil on which the Bi-plated film is formed. It should be noted that the manganese-plating bath used in the production of the Mn-plated film is not particularly limited and can be appropriately selected from known manganese-plating baths that can precipitate a single Mn thin film. For example, when a sulfate bath is selected as the manganese-plating bath, as an example, a plating bath produced as follows can be used: manganese sulfate as a soluble manganese salt is added to a 1.0 mol / L aqueous solution of ammonium sulfate so that Mn 2+ The ion concentration is 0.92 mol / L, thereby producing the manganese plating bath. In addition, additives and the like may be added to the manganese plating bath.
[0122] The current density applied during electroplating is not particularly limited, and can be appropriately set in consideration of, for example, the plating bath used and the material of the current collector used as the substrate.
[0123] Next, the copper foil and the plating layer (i.e., Bi-plated film and Mn-plated film) formed on the copper foil are heated. Through this heat treatment, Mn is diffused from the solid phase of the Mn-plated film into the Bi-plated film, and Cu is further diffused from the solid phase of the copper foil into the Bi-plated film, and an active material layer 104 composed of an alloy film containing Bi and Mn can be produced. The copper foil, Bi-plated film, and Mn-plated film laminate obtained by electroplating the Bi-plated film and the Mn-plated film on the copper foil are subjected to heat treatment for more than 30 minutes and less than 100 hours at a temperature of more than 150° C. in a non-oxidizing atmosphere, so that Mn is diffused from the solid phase of the Mn-plated film into the Bi-plated film, and Cu is further diffused from the solid phase of the copper foil into the Bi-plated film, and an active material layer 104 composed of, for example, a BiMn film or a Bi4Mn3Cu4 film can be produced.
[0124] For example, for a sample in which bismuth is electroplated on a copper foil with a target thickness of 3 μm and manganese is further electroplated thereon with a target thickness of 1 μm, a heat treatment is performed for 100 hours at a temperature of 200°C in an argon atmosphere to produce an active material layer composed of a thin film containing BiMn. In addition, for the prepared active material layer composed of a thin film containing BiMn, a surface structure analysis is also performed based on surface X-ray diffraction measurement. The X-ray diffraction measurement is performed as follows: From the surface of the active material layer, that is, in the thickness direction of the active material layer, an X-ray diffraction device (manufactured by RIGAKU, MiNi Flex) is used to diffract the active material layer using a wavelength of 100 nm. and The θ-2θ method was performed using Cu-Kα rays as X-rays. The obtained X-ray diffraction pattern was the same as the X-ray diffraction pattern of the first electrode prepared in Example 1 described later, which is equivalent to Figure 3The X-ray diffraction pattern of "Initial" among the X-ray diffraction patterns shown in FIG. BiMn whose space group as a crystal structure belongs to P63 / mmc, and Cu foil as a current collector and Cu phases contained in the active material layer were identified.
[0125] In addition, similarly, for a sample in which bismuth was electroplated on copper foil with a target thickness of 4 μm and manganese was further electroplated thereon with a thickness of 1 μm, a heat treatment was performed for 100 hours at a temperature of 200°C in an argon atmosphere to produce an active material layer composed of a thin film containing Bi4Mn3Cu4. In addition, for the prepared active material layer composed of a thin film containing Bi4Mn3Cu4, a surface structure analysis was also performed based on surface X-ray diffraction measurement. The X-ray diffraction measurement was performed as follows: From the surface of the active material layer, that is, in the thickness direction of the active material layer, an X-ray diffraction device (manufactured by RIGAKU, MiNi Flex) was used to diffract at a wavelength of 1.5 Å. and The θ-2θ method was performed using Cu-Kα rays as X-rays. The obtained X-ray diffraction pattern was the same as the X-ray diffraction pattern of the first electrode prepared in Example 4 described later, which is equivalent to Figure 7 The X-ray diffraction pattern of "Initial" among the X-ray diffraction patterns shown in FIG. Bi4Mn3Cu4, whose space group belongs to Fm-3m as a crystal structure, and the phase of Cu foil as a current collector were identified.
[0126] When the active material layer 104 is a heat-treated plating layer produced by the above-mentioned method, the active material layer 104 can have, for example, the following high density. For example, when the active material layer 104 is composed of a BiMn thin film produced by the above-mentioned plating method, the active material layer 104 can have, for example, a density of 5.8 g / cm 3 Above 9.44g / cm 3 The density can also be 7.2g / cm 3 Above 9.44g / cm 3 For example, when the active material layer 104 is composed of a Bi4Mn3Cu4 thin film produced by the above-mentioned plating method, the active material layer 104 may have a density of 5.8 g / cm 3 Above and 9.51g / cm 3 The density can also be 7.2g / cm 3 Above 9.51g / cm 3 The following density.
[0127] Hereinafter, each structure of the battery 1000 of this embodiment will be described in more detail, taking as an example a case where the first electrode 101 is a negative electrode and the second electrode 103 is a positive electrode.
[0128] [First electrode]
[0129] As described above, the first electrode 101 has a current collector 100 and an active material layer 104. The active material layer 104 is configured as described above. The first electrode 101 functions as a negative electrode. Therefore, the active material layer 104 contains a negative electrode active material having the property of storing and releasing lithium ions. The active material layer 104 contains an alloy containing Bi and Mn. The alloy containing Bi and Mn is, for example, BiMn having a crystal structure of space group P63 / mmc or Bi4Mn3Cu4 having a space group Fm-3m. BiMn and Bi4Mn3Cu4 function as negative electrode active materials.
[0130] Bi is a metal element that alloys with lithium. On the other hand, Mn and Cu do not alloy with lithium, so it is speculated that alloys containing Bi and Mn, and alloys containing Bi, Mn and Cu, when lithium atoms are extracted and embedded during charging and discharging, reduce the load of the negative electrode active material on the crystal structure, and the reduction in the capacity retention rate of the battery is suppressed. For example, when BiMn functions as a negative electrode active material, Bi forms an alloy with lithium during charging, thereby absorbing and storing lithium. That is, in the active material layer 104, when the battery 1000 is charged, a lithium-bismuth alloy is generated. The generated lithium-bismuth alloy, for example, includes at least one selected from the group consisting of LiBi and Li3Bi. That is, when the battery 1000 is charged, the active material layer 104, for example, includes at least one selected from the group consisting of LiBi and Li3Bi. When the battery 1000 is discharged, lithium is released from the lithium-bismuth alloy, and the lithium-bismuth alloy is restored to BiMn.
[0131] BiMn as the negative electrode active material reacts, for example, as follows during charge and discharge of the battery 1000. The following reaction examples are examples when the lithium-bismuth alloy generated during charge is Li3Bi.
[0132] Charging: BiMn+3Li + +3e - →Li3Bi+Ni
[0133] Discharge: Li3Bi+Mn→BiMn+3Li + +3 -
[0134] The active material layer 104 may substantially contain only BiMn as an active material. In this case, the battery 1000 may have an increased capacity and improved cycle characteristics in addition to improved energy efficiency. It should be noted that "the active material layer 104 substantially contains only BiMn as an active material" means, for example, that the active material other than BiMn in the active material contained in the active material layer 104 is 1% by mass or less. The active material layer 104 may contain only BiMn as an active material.
[0135] For example, when Bi4Mn3Cu4 functions as a negative electrode active material, Bi forms an alloy with lithium during charging, thereby absorbing lithium. That is, in the active material layer 104, when the battery 1000 is charged, a lithium-bismuth alloy is generated. The generated lithium-bismuth alloy, for example, includes at least one selected from the group consisting of LiBi and Li3Bi. That is, when the battery 1000 is charged, the active material layer 104, for example, includes at least one selected from the group consisting of LiBi and Li3Bi. When the battery 1000 is discharged, lithium is released from the lithium-bismuth alloy, and the lithium-bismuth alloy is restored to Bi4Mn3Cu4.
[0136] Bi4Mn3Cu4 as the negative electrode active material reacts as follows during charging and discharging of the battery 1000. It should be noted that the following reaction examples are examples in which the lithium-bismuth alloy generated during charging is Li3Bi.
[0137] Charging: Bi4Mn3Cu4+12Li + +12e - →4Li3Bi+3Mn+4Cu
[0138] Discharge: 4Li3Bi+3Mn+4Cu→Bi4Mn3Cu4+12Li + +12e -
[0139] The active material layer 104 may substantially contain only Bi4Mn3Cu4 as an active material. In this case, the battery 1000 has an improved capacity and improved cycle characteristics in addition to improved energy efficiency. It should be noted that "the active material layer 104 substantially contains only Bi4Mn3Cu4 as an active material" means, for example, that among the active materials contained in the active material layer 104, other active materials other than Bi4Mn3Cu4 are less than 1% by mass. The active material layer 104 may contain only Bi4Mn3Cu4 as an active material.
[0140] The active material layer 104 may not contain a solid electrolyte. For example, the active material layer 104 may be a layer formed of an alloy containing Bi and Mn and / or a lithium-bismuth alloy generated during charging. The alloy containing Bi and Mn may be at least one selected from the group consisting of BiMn and Bi4Mn3Cu4.
[0141] The active material layer 104 may be disposed in direct contact with the surface of the current collector 100 .
[0142] The active material layer 104 may be in a thin film form.
[0143] The active material layer 104 may be a heat-treated plating layer. The active material layer 104 may be a heat-treated plating layer provided in direct contact with the surface of the current collector 100. That is, as described above, the active material layer 104 may be a layer formed by heat-treating a Bi-plated film formed on the current collector 100 and a Mn-plated film formed on the Bi-plated film. The current collector 100 may contain Cu, for example.
[0144] If the active material layer 104 is a heat-treated plating layer that is directly in contact with the surface of the current collector 100, the active material layer 104 is firmly bonded to the current collector 100. As a result, the deterioration of the current collection characteristics of the first electrode 101 caused by repeated expansion and contraction of the active material layer 104 can be further suppressed. Therefore, the cycle characteristics of the battery 1000 are further improved. Furthermore, if the active material layer 104 is a heat-treated plating layer, Bi alloyed with lithium is contained in the active material layer 104 at a high density, so that further high capacity can be achieved.
[0145] The active material layer 104 may contain a material other than the alloy containing Bi and Mn.
[0146] The active material layer 104 may further include a conductive material.
[0147] As the conductive material, carbon materials, metals, inorganic compounds and conductive polymers can be mentioned. As carbon materials, graphite, acetylene black, carbon black, Ketjen black, carbon whiskers, needle coke and carbon fiber can be mentioned. As graphite, natural graphite and artificial graphite can be mentioned. As natural graphite, block graphite and flaky graphite can be mentioned. As metals, copper, nickel, aluminum, silver and gold can be mentioned. As inorganic compounds, tungsten carbide, titanium carbide, tantalum carbide, molybdenum carbide, titanium boride and titanium fluoride can be mentioned. These materials can be used alone or in combination.
[0148] The active material layer 104 may further include a binder.
[0149] As the binder, fluorine-containing resin, thermoplastic resin, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, and natural butyl rubber (NBR) can be cited. As fluorine-containing resin, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), and fluororubber can be cited. As thermoplastic resin, polypropylene and polyethylene can be cited. These materials can be used alone or in combination.
[0150] The thickness of the active material layer 104 is not particularly limited, and may be, for example, 1 μm or more and 100 μm or less.
[0151] The material of the current collector 100 is, for example, a single metal or an alloy. More specifically, it may be a single metal or an alloy containing at least one selected from the group consisting of copper, chromium, nickel, titanium, platinum, gold, aluminum, tungsten, iron, and molybdenum. The current collector 100 may also be stainless steel.
[0152] The current collector 100 may include copper (Cu). By including Cu, the current collector 100 is used as a substrate, a Bi-plated film and a Mn-plated film are formed on the substrate, and then heat-treated, so that the active material layer 104 containing an alloy including Bi, Mn, and Cu such as Bi4Mn3Cu4 can be easily formed.
[0153] The current collector 100 may be a laminated film.
[0154] [Electrolyte layer]
[0155] The electrolyte layer 102 includes an electrolyte material. The electrolyte layer 102 is composed of, for example, a non-aqueous electrolyte. The electrolyte material contained in the electrolyte layer 102 may be a solid electrolyte or may include an electrolyte solution. It should be noted that Figure 1 2 shows a configuration example in which the electrolyte layer 102 is a solid electrolyte.
[0156] When the electrolyte material is a solid electrolyte, as the solid electrolyte, a halide solid electrolyte, a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, or a complex hydride solid electrolyte can be used.
[0157] A halide solid electrolyte is a solid electrolyte containing a halogen element. A halide solid electrolyte contains not only a halogen element but also oxygen. A halide solid electrolyte does not contain sulfur (S).
[0158] The halide solid electrolyte may be, for example, a material represented by the following composition formula (1).
[0159] Li α M β X γ …Formula (1)
[0160] Here, α, β, and γ are values greater than 0, M is at least one selected from the group consisting of metal elements and semi-metal elements other than Li, and X is at least one selected from the group consisting of F, Cl, Br, and I.
[0161] “Semi-metallic elements” refer to: B, Si, Ge, As, Sb and Te.
[0162] "Metallic elements" refer to all elements included in Groups 1 to 12 of the periodic table except hydrogen, and all elements included in Groups 13 to 16 except B, Si, Ge, As, Sb, Te, C, N, P, O, S and Se. In other words, they are a group of elements that can become cations when forming inorganic compounds with halogen compounds.
[0163] In the composition formula (1), M may include Y, and X may include Cl and Br.
[0164] As halide solid electrolytes, for example, Li3(Ca, Y, Gd)X6, Li2MgX4, Li2FeX4, Li(Al, Ga, In)X4, Li3(Al, Ga, In)X6, LiI, etc. can be used. Here, in these solid electrolytes, the element X is at least one selected from the group consisting of F, Cl, Br and I. It should be noted that in the present disclosure, when an element in the expression formula is represented as "(Al, Ga, In)", the expression represents at least one element selected from the group of elements in brackets. That is, "(Al, Ga, In)" has the same meaning as "at least one selected from the group consisting of Al, Ga and In". The same applies to other elements.
[0165] Another example of a halide solid electrolyte is Li a Me b Y c A compound represented by X6. Here, a+mb+3c=6 and c>0 are satisfied. Me is at least one selected from the group consisting of metal elements and semi-metal elements other than Li and Y. m represents the valence of Me. "Semi-metal elements" refer to: B, Si, Ge, As, Sb and Te. "Metal elements" refer to: all elements contained in Groups 1 to 12 of the periodic table (excluding hydrogen), and all elements contained in Groups 13 to 16 of the periodic table (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S and Se).
[0166] In order to improve the ion conductivity of the halide solid electrolyte material, Me can be at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta and Nb. The halide solid electrolyte can be Li3YCl6, Li3YBr6 or Li3YBr p Cl 6-p It should be noted that p satisfies 0 <p<6。
[0167] The sulfide solid electrolyte refers to a solid electrolyte containing sulfur (S). The sulfide solid electrolyte may contain not only sulfur but also a halogen element.
[0168] As sulfide solid electrolytes, for example, Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4 or Li 10 GeP2S 12 wait.
[0169] As oxide solid electrolytes, for example, NASICON solid electrolytes represented by LiTi2(PO4)3 and its element substitution products, (LaLi)TiO3-based perovskite solid electrolytes, and Li 14 ZnGe4O 16 , LISICON type solid electrolyte represented by Li4SiO4, LiGeO4 and their element substitution products, Li7La3Zr2O 12 Garnet-type solid electrolytes represented by Li3PO4 and its element substitution bodies, Li3PO4 and its N substitution bodies, and glass or glass ceramics based on Li-BO compounds such as LiBO2 and Li3BO3 and added with Li2SO4, Li2CO3, etc.
[0170] As a polymer solid electrolyte, for example, a compound of a polymer compound and a lithium salt can be used. The polymer compound can have an ethylene oxide structure. The polymer compound having an ethylene oxide structure can contain a large amount of lithium salt. Therefore, the ion conductivity can be further improved. As lithium salts, LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) and LiC(SO2CF3)3 can be used. One lithium salt selected from the exemplified lithium salts can be used alone. Alternatively, a mixture of two or more lithium salts selected from the exemplified lithium salts can be used.
[0171] As the coordinated hydride solid electrolyte, for example, LiBH4-LiI, LiBH4-P2S5, etc. can be used.
[0172] The electrolyte layer 102 may include a halide solid electrolyte. The halide solid electrolyte does not contain sulfur.
[0173] The electrolyte layer 102 may not contain a sulfide solid electrolyte.
[0174] The electrolyte layer 102 may be composed of only a halide solid electrolyte. It should be noted that "substantially" in this specification means that the electrolyte layer 102 may be composed of only a halide solid electrolyte. The electrolyte layer 102 may be composed of only a halide solid electrolyte.
[0175] According to the above configuration, the ion conductivity of the electrolyte layer 102 can be improved. This can reduce the decrease in the energy density of the battery.
[0176] The electrolyte layer 102 may further include a binder. As the binder, the same material as that used in the active material layer 104 can be used.
[0177] The electrolyte layer 102 may have a thickness of 1 μm or more and 500 μm or less. When the electrolyte layer 102 has a thickness of 1 μm or more, the first electrode 101 and the second electrode 103 are less likely to short-circuit. When the electrolyte layer 102 has a thickness of 500 μm or less, the battery can operate at high power.
[0178] The shape of the solid electrolyte is not particularly limited. When the solid electrolyte is a powder material, its shape may be, for example, needle-shaped, spherical, ellipsoidal, etc. For example, the solid electrolyte may be in the form of particles.
[0179] For example, when the solid electrolyte is in the form of particles (e.g., spheres), the median particle size of the solid electrolyte may be 100 μm or less, or 10 μm or less.
[0180] In the present disclosure, the “median diameter” refers to the particle diameter at which the cumulative volume in the volume-based particle size distribution is equivalent to 50%. The volume-based particle size distribution is measured, for example, using a laser diffraction measuring device or an image analyzer.
[0181] The solid electrolyte contained in the electrolyte layer 102 can be produced according to the following method.
[0182] The raw material powder is prepared so as to have a target composition. Examples of the raw material powder are oxides, hydroxides, halides or acyl halides.
[0183] As an example, when the target composition is Li3YBr4Cl2, LiBr, YCl and YBr are mixed at a molar ratio of about 3:0.66:0.33. The raw material powders can be mixed at a pre-adjusted molar ratio in order to offset composition changes that may occur during the synthesis process.
[0184] The raw powders are reacted with each other in a mechanochemical manner (i.e., by a mechanochemical grinding method) in a mixing device such as a planetary ball mill to obtain a reactant. The reactant can be calcined in a vacuum or in an inert atmosphere. Alternatively, the mixture of the raw powders can be calcined in a vacuum or in an inert atmosphere to obtain a reactant. The calcination is preferably performed at a temperature of 100° C. to 300° C. for more than 1 hour. In order to suppress the composition change during calcination, the raw powder is preferably calcined in a closed container such as a quartz tube.
[0185] According to these methods, the solid electrolyte used in the electrolyte layer 102 is obtained.
[0186] Figure 2 1 is a cross-sectional view schematically showing a modified example of a battery according to an embodiment of the present disclosure. When the electrolyte material constituting the electrolyte layer 102 is an electrolyte solution, that is, when the electrolyte layer contains an electrolyte solution, the battery according to an embodiment of the present disclosure may be, for example, Figure 2 The battery 2000 of the above structure. It should be noted that Figure 2 In Figure 1 The components shown have the same functions and are marked with the same symbols. The battery 2000 includes: a first electrode 101, a second electrode 103, an electrolyte 201, a separator 202, and a housing 203. The separator 202 is located between the first electrode 101 and the second electrode 103. The first electrode 101 and the second electrode 103 are opposite to each other via the separator 202. The first electrode 101, the second electrode 103, the separator 202, and the electrolyte 201 are accommodated in the housing 203. The electrolyte 201 is, for example, an electrolyte impregnated in the first electrode 101, the second electrode 103, and the separator 202. In this way, in the battery 2000 having a structure using an electrolyte as an electrolyte, the electrolyte 201 impregnated in the separator 202 is located between the first electrode 101 and the second electrode 103. That is, the electrolyte 201 impregnated in the separator 202 in this way becomes an electrolyte layer. The electrolyte 201 may also fill the inner space of the housing 203 .
[0187] The electrolyte solution 201 contains, for example, a non-aqueous solvent and a lithium salt.
[0188] Examples of non-aqueous solvents are cyclic carbonate solvents, chain carbonate solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents or fluorine solvents. Examples of cyclic carbonate solvents are ethylene carbonate, propylene carbonate, butylene carbonate or vinylene carbonate. Examples of chain carbonate solvents are dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate. Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dioxane or 1,3-dioxolane. Examples of chain ether solvents are 1,2-dimethoxyethane or 1,2-diethoxyethane. Examples of cyclic ester solvents are γ-butyrolactone. Examples of chain ester solvents are methyl acetate. Examples of fluorine solvents are fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, ethyl fluoromethyl carbonate or dimethylene fluorocarbonate. One non-aqueous solvent selected from them can be used alone. Alternatively, a mixture of two or more non-aqueous solvents selected from them can be used. The electrolyte may contain vinylene carbonate as a solvent.
[0189] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.
[0190] The separator 202 has lithium ion conductivity. The material of the separator 202 is not particularly limited as long as it allows lithium ions to pass through. The material of the separator 202 can be at least one selected from the group consisting of a solid electrolyte, a gel electrolyte, an ion exchange resin membrane such as a lithium cation exchange resin, a semipermeable membrane, and a porous membrane. If the separator 202 is made of these materials, the safety of the battery 2000 can be fully ensured. Examples of the solid electrolyte include sulfide solid electrolytes such as Li2S-P2S5, Li7La3Zr2O 12 As the gel electrolyte, there can be mentioned a gel electrolyte containing a fluororesin such as PVdF. As the ion exchange resin membrane, there can be mentioned a cation exchange membrane, an anion exchange membrane, etc. As the porous membrane, there can be mentioned a porous membrane made of a polyolefin resin, a porous membrane formed by weaving glass fiber into a non-woven fabric, etc.
[0191] The outer casing 203 is made of a material obtained by laminating a metal foil such as aluminum foil with a resin film such as polyethylene terephthalate (PET) film, for example. The outer casing 203 may be a container made of resin or metal.
[0192] The electrolyte material used in the electrolyte layer is not limited to the above-mentioned solid electrolyte or electrolyte solution, and a gel electrolyte or an ionic liquid may also be used.
[0193] As the gel electrolyte, a polymer material impregnated with a non-aqueous electrolyte can be used. Examples of the polymer material are polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.
[0194] Examples of cations contained in ionic liquids are:
[0195] (i) Aliphatic chain quaternary salts such as tetraalkylammonium or tetraalkylphosphonium;
[0196] (ii) an aliphatic cyclic ammonium such as a pyrrolidinium, morpholinium, imidazolinium, tetrahydropyridinium, piperazinium or piperidinium; or
[0197] (iii) Nitrogen-containing heterocyclic aromatic cations such as pyridinium and imidazolium cations.
[0198] An example of an anion contained in an ionic liquid is PF6 - 、BF4 - 、SbF6 - 、AsF6 - 、SO3CF3 - 、N(SO2CF3)2 - 、N(SO2C2F5)2 - 、N(SO2CF3)(SO2C4F9) - or C(SO2CF3)3 - .
[0199] The ionic liquid may contain a lithium salt.
[0200] [Second electrode]
[0201] The second electrode 103 functions as a positive electrode. The second electrode 103 contains a material that can absorb and release metal ions such as lithium ions. This material is, for example, a positive electrode active material.
[0202] The second electrode 103 may include a current collector 105 and an active material layer 106. The active material layer 106 includes a positive electrode active material and is disposed between the current collector 105 and the electrolyte layer 102, for example.
[0203] The active material layer 106 may be disposed on the surface of the current collector 105 in direct contact with the current collector 105 .
[0204] As the positive electrode active material, for example, a lithium-containing transition metal oxide, a transition metal fluoride, a polyanion material, a fluorinated polyanion material, a transition metal sulfide, a transition metal oxysulfide, or a transition metal oxynitride can be used. Examples of lithium-containing transition metal oxides include LiNi1-x-y Co x Al y O2((x+y)<1), LiNi 1-x-y Co x Mn y O2 ((x+y)<1) or LiCoO2, etc. In particular, when a lithium-containing transition metal oxide is used as the positive electrode active material, the manufacturing cost of the electrode can be reduced and the average discharge voltage of the battery can be increased. For example, the positive electrode active material can include Li(Ni, Co, Mn)O2.
[0205] Examples of the material of the current collector 105 include metal materials, such as copper, stainless steel, iron, and aluminum.
[0206] The second electrode 103 may include a solid electrolyte. As the solid electrolyte, the solid electrolytes exemplified as the material constituting the electrolyte layer 102 may be used.
[0207] The positive electrode active material may have a median particle size of 0.1 μm or more and 100 μm or less. When the positive electrode active material has a median particle size of 0.1 μm or more, the positive electrode active material and the solid electrolyte can form a good dispersion state. As a result, the charge and discharge characteristics of the battery are improved. When the positive electrode active material has a median particle size of 100 μm or less, the lithium diffusion rate is increased. As a result, the battery can operate at high power.
[0208] The positive electrode active material may have a larger median particle size than the solid electrolyte, thereby allowing the positive electrode active material and the solid electrolyte to form a well-dispersed state.
[0209] From the viewpoint of battery energy density and power, in the second electrode 103 , the ratio of the volume of the positive electrode active material to the total volume of the positive electrode active material and the volume of the solid electrolyte may be 0.30 or more and 0.95 or less.
[0210] In order to prevent the solid electrolyte from reacting with the positive electrode active material, a covering layer can be formed on the surface of the positive electrode active material. Thus, the increase in the reaction overvoltage of the battery can be suppressed. Examples of the covering material contained in the covering layer are sulfide solid electrolytes, oxide solid electrolytes, or halide solid electrolytes.
[0211] The thickness of the second electrode 103 may be 10 μm or more and 500 μm or less. When the thickness of the second electrode 103 is 10 μm or more, sufficient battery energy density can be ensured. When the thickness of the second electrode 103 is 500 μm or less, the battery can operate at high power.
[0212] For the purpose of improving electron conductivity, the second electrode 103 may include a conductive material.
[0213] The second electrode 103 may include a binder.
[0214] As the conductive material and the binder, the same materials as those that can be used for the active material layer 104 can be used.
[0215] The second electrode 103 may contain a non-aqueous electrolyte, a gel electrolyte, or an ionic liquid in order to facilitate the transfer of lithium ions and improve the power characteristics of the battery.
[0216] In the above description, an example of a configuration in which the first electrode 101 is a negative electrode and the second electrode 103 is a positive electrode has been described. However, the first electrode 101 may be a positive electrode and the second electrode 103 may be a negative electrode.
[0217] When the first electrode 101 is a positive electrode and the second electrode 103 is a negative electrode, the active material layer 104 is a positive electrode active material layer. That is, Bi contained in the active material layer 104 functions as a positive electrode active material. In this case, the second electrode 103 as a negative electrode is composed of lithium metal, for example.
[0218] The battery 1000 is basically composed of a first electrode 101, an electrolyte layer 102, and a second electrode 103, and is sealed in a sealed container so that air and moisture are not mixed in. The shape of the battery 1000 can be coin-shaped, cylindrical, square, sheet-shaped, button-shaped, flat, and stacked.
[0219] Example
[0220] The following examples and reference examples are used to describe the details of the present disclosure. The following examples are examples, and the present disclosure is not limited to the following examples.
[0221] (Example 1)
[0222] <Fabrication of First Electrode>
[0223] As a pre-treatment, the copper foil (10cm×10cm, thickness: 10μm) is pre-degreased with an organic solvent, and then one side is masked and immersed in an acidic solvent to degrease and activate the surface of the copper foil. The electroplating of bismuth on the copper foil is carried out as follows: the copper foil that becomes the plating substrate is immersed in a bismuth plating bath, and a circuit is formed in a way that the copper foil becomes an anode from an external power supply, and the current and potential are adjusted. As a result, the bismuth ions in the bismuth plating bath are reduced on the copper foil to form a Bi-plated film. Next, the copper foil electroplated with bismuth is immersed in a manganese plating bath, and a circuit is formed in a way that the copper foil electroplated with bismuth becomes an anode from an external power supply, and the current and potential are adjusted. As a result, the manganese ions in the manganese plating bath are reduced on the bismuth plating to form a Mn-plated film.
[0224] As a bismuth plating bath, an organic sulfonic acid bath was used. The bismuth plating bath was prepared as follows: Bi 3+ The bismuth methanesulfonate was added as a soluble bismuth salt so that the ion became 0.18 mol / L.
[0225] A sulfate bath was selected as the manganese plating bath. The manganese plating bath was prepared as follows: Mn 2+ Manganese sulfate as a soluble manganese salt was added so that the ion became 0.92 mol / L, and it was produced by heat.
[0226] The activated copper foil was connected to a power source in a way that current could be applied, and then immersed in a bismuth plating bath. Then, the current density was controlled to 2A / dm 2 Thus, bismuth was electroplated on the unmasked copper foil surface in a manner to have a thickness of approximately 3 μm, thereby producing a Bi-plated film.
[0227] Next, the copper foil with the Bi-plated film was connected to a power source in a manner that allows current to be applied, similar to the bismuth electroplating, and then immersed in a manganese plating bath. The current density was then controlled to 2 A / dm 2 Thus, manganese was electroplated on the unmasked copper foil surface in a manner to have a thickness of approximately 1 μm, thereby producing a Mn plated film.
[0228] In addition, in the step of immersing the copper foil in the plating bath, masking was performed on the surface other than the plated surface.
[0229] After electroplating, the copper foil was recovered from the plating bath, removed from the mask, cleaned with pure water and dried. Thereafter, the copper foil and the plating layers (i.e., the Bi plating film and the Mn plating film) formed on the copper foil were heat treated at 200° C. for 100 hours in an electric furnace with an argon atmosphere.
[0230] It should be noted that the coating after heat treatment is equivalent to the active material layer of the first electrode. The structure of the coating after heat treatment, i.e., the active material layer, was analyzed based on surface X-ray diffraction measurement. The X-ray diffraction measurement was performed as follows: From the surface of the active material layer, i.e., the thickness direction of the active material layer, an X-ray diffraction device (made by RIGAKU, MiNi Flex) was used with a wavelength of and The θ-2θ method was performed using Cu-Kα rays as X-rays. Figure 3 The graphs show X-ray diffraction patterns of the active material layer of the first electrode in the battery of Example 1 at the initial stage, after charge, and after charge and discharge. Figure 3In the X-ray diffraction pattern of the initial active material layer, the X-ray diffraction pattern is indicated as "Initial". From this X-ray diffraction pattern, it is confirmed that BiMn with a hexagonal crystal structure and a space group belonging to P63 / mmc is generated in the active material layer. It should be noted that the Cu foil as the collector and the Cu phase contained in the active material layer are also confirmed in the X-ray diffraction pattern.
[0231] Thereafter, the sheet was punched out into a size of 2×2 cm to obtain a first electrode. That is, the first electrode of Example 1 had a structure in which an active material layer composed of BiMn was provided on a current collector composed of copper foil.
[0232] <Battery production>
[0233] The first electrode is used as the working electrode. A Li metal with a thickness of 0.34 μm is used as the counter electrode. The Li metal is obtained by double covering a microporous separator Cellcard (3401) manufactured by Cellcard. As an electrolyte, a solution obtained by dissolving LiPF6 in vinyl carbonate (VC) at a concentration of 1.0 mol / L is prepared. Using this working electrode, counter electrode, and electrolyte, a battery as a test cell of Example 1 is assembled. It should be noted that the test cell prepared here is a test cell for single-electrode evaluation using a working electrode and a counter electrode, which is used to test the performance of one pole of the electrode in the battery. In detail, the electrode of the test object is used in the working electrode, and a sufficient amount of appropriate active material is supplied to the counter electrode for the reaction of the working electrode. This test cell is used to test the performance of the negative electrode as the first electrode, so as to use it normally, a large excess of Li metal is used as the counter electrode. The first electrode whose performance is tested using this test cell is combined with a positive electrode containing the positive electrode active material described in the above embodiment, such as a transition metal oxide containing Li, so that it can be used as a negative electrode.
[0234] <Charge and discharge test>
[0235] The battery made as the test battery unit was subjected to a charge and discharge test. In the charge and discharge test, the battery was charged to 0 V (Li reference) at a constant current value of 0.06 mA (the theoretical capacity of Bi at a rate of 384 mAh / g is equivalent to 0.05 IT), and discharged to 2.0 V (Li reference), and the charge and discharge were repeated. The battery was tested in a thermostatic chamber set at 25°C. Figure 4 Graph showing the results of the charge and discharge test of the battery of Example 1. Figure 4 As shown, in Example 1, the charge reaction potential changes from 0.5 to 0.8 V (vs. Li), and the discharge reaction potential becomes approximately 0.85 V (vs. Li).
[0236] <Structural changes of active materials based on X-ray diffraction>
[0237] For the first electrode charged and discharged in the same procedure as the charge and discharge test conditions shown in the above "Charge and Discharge Test", after charging and after charging and discharging, X-ray diffraction measurement is performed on the surface where the active material layer is formed. The X-ray diffraction measurement of the active material layer after charging and charging and discharging is performed in the same manner as the X-ray diffraction measurement performed on the above-mentioned initial active material layer. Figure 3 In the X-ray diffraction pattern of the active material layer after charge is the X-ray diffraction pattern indicated as "charge", and the X-ray diffraction pattern of the active material layer after charge-discharge is the X-ray diffraction pattern indicated as "charge-discharge". Figure 3 The X-ray diffraction pattern shown can confirm that BiMn forms Li3Bi by charging and forms BiMn again by discharging.
[0238] (Example 2)
[0239] <Fabrication of First Electrode>
[0240] The first electrode was manufactured in the same manner as in Example 1 except that the final size of the first electrode was different. In Example 2, the first electrode was punched into size.
[0241] <Solid Electrolyte>
[0242] As a solid electrolyte constituting the electrolyte layer, a sulfide solid electrolyte Li6PS5Cl (produced by Ampcera, 80 mg) was used.
[0243] <Battery production>
[0244] The obtained first electrode is arranged in an insulating outer cylinder having an inner diameter of 9.4 mm. On the active material layer of the first electrode, a solid electrolyte Li6PS5Cl (80 mg) is stacked, and then an indium-lithium alloy (molar ratio: In:Li=1:1) (200 mg) is stacked as the second electrode to obtain a stack. The indium-lithium alloy is made as follows: a small piece of lithium foil is crimped on the indium foil to diffuse lithium into the indium. For the above-mentioned stack, a pressure of 360 MPa is applied in the stacking direction to form a battery as a test battery cell having a first electrode, a solid electrolyte layer and a second electrode. In the battery as a test battery cell, the thickness of the first electrode is 1.5 μm, the thickness of the solid electrolyte layer is 500 μm, and the thickness of the second electrode is 15 μm.
[0245] Next, a current collector made of stainless steel was attached to the first electrode and the second electrode, and a current collecting lead was attached to the current collector.
[0246] Finally, an insulating nozzle is used to block the inside of the insulating outer cylinder from the external gas atmosphere, thereby hermetically sealing the inside of the cylinder.
[0247] As described above, a battery as a test cell of Example 2 was obtained, in which the first electrode including the active material layer formed of BiMn was used as the working electrode and the lithium-indium alloy was used as the counter electrode.
[0248] <Charge and discharge test>
[0249] The battery was charged and discharged under the following conditions. The theoretical capacity of Bi was 384 mAh / g based on the weight of Bi after electroplating. The battery was charged to -0.62 V (i.e., 0 V (vs. Li+ / Li)) at a constant current value of 0.05 IT based on the Bi rate. The battery was then discharged to 1.38 V (i.e., 2.0 V (vs. Li+ / Li)). The battery was then charged to -0.62 V (i.e., 0 V (vs. Li+ / Li)). The battery was tested in a thermostatic chamber at 25°C. Figure 5 : is a graph showing the results of the charge and discharge test of the battery of Example 2. Figure 5 When the InLi-based potential shown is converted to the Li-based potential, in Example 2, the charge reaction potential changes from 0.5 to 0.77 V (vs. Li), and the discharge reaction potential becomes around 0.83 V (vs. Li). Figure 5 The potential of the graph shown is the potential of InLi reference when the counter electrode is InLi. The conversion of the potential of the InLi reference to the potential of the Li reference is obtained by converting the InLi potential to +0.62V based on the Li reference. In the following embodiments, when InLi is used as the counter electrode, the potential can also be converted to the Li reference in the same way.
[0250] (Example 3)
[0251] <Fabrication of First Electrode>
[0252] The first electrode was manufactured in the same manner as in Example 1 except that the final size of the first electrode was different. In Example 3, the first electrode was punched into size.
[0253] <Production of solid electrolyte>
[0254] In an argon atmosphere with a dew point below -60°C (hereinafter referred to as "dry argon atmosphere"), LiBr, YCl3 and YBr3 are prepared as raw material powders in a molar ratio of LiBr:YCl3:YBr3=3:2 / 3:1 / 3. These raw material powders are crushed and mixed in a mortar to obtain a mixed powder. Then, the obtained mixture of raw material powders is calcined in a dry argon atmosphere at 500°C for 3 hours in an electric furnace. The obtained calcined product is crushed in a mortar with a rod. In this way, a solid electrolyte having a composition of Li3YBr4Cl2 is obtained.
[0255] <Battery production>
[0256] In the preparation of the solid electrolyte layer, a battery as a test battery cell of Example 3 was prepared in the same manner as in Example 2, except that Li3YBr4Cl2 (80 mg) was used instead of the solid electrolyte Li6PS5Cl (80 mg).
[0257] <Charge and discharge test>
[0258] The battery was charged and discharged under the following conditions. The theoretical capacity of Bi was 384 mAh / g based on the weight of Bi after electroplating. The battery was charged to -0.42 V (i.e., 0.2 V (vs. Li+ / Li)) at a constant current value of 0.05 IT based on the Bi rate. The battery was then discharged to 1.38 V (i.e., 2.0 V (vs. Li+ / Li)). The battery was then charged to -0.42 V (i.e., 0.2 V (vs. Li+ / Li)). The battery was tested in a thermostatic chamber at 25°C. Figure 6 : is a graph showing the results of the charge and discharge test of the battery of Example 3. Figure 6 When the InLi-based potential shown is converted to the Li-based potential, in Example 3, the charge reaction potential in the second cycle and thereafter becomes 0.79 V (vs. Li) from 0.5, and the discharge reaction potential becomes approximately 0.85 V (vs. Li).
[0259] (Example 4)
[0260] <Fabrication of First Electrode>
[0261] As a pre-treatment, the copper foil (10cm×10cm, thickness: 10μm) is pre-degreased with an organic solvent, and then one side is masked and immersed in an acidic solvent to degrease and activate the surface of the copper foil. The electroplating of bismuth on the copper foil is carried out as follows: the copper foil that becomes the plating substrate is immersed in a bismuth plating bath, and a circuit is formed in a way that the copper foil from an external power supply becomes the anode, and the current and potential are adjusted. As a result, the bismuth ions in the bismuth plating bath are reduced on the copper foil to form a Bi-plated film. Next, the copper foil electroplated with bismuth is immersed in a manganese plating bath, and a circuit is formed in a way that the copper foil electroplated with bismuth from an external power supply becomes the anode, and the current and potential are adjusted. As a result, the manganese ions in the manganese plating bath are reduced on the bismuth plating to form a Mn-plated film.
[0262] An organic sulfonic acid bath was used as a bismuth plating bath. The bismuth plating bath was prepared as follows: Bi 3+ The bismuth methanesulfonate was added as a soluble bismuth salt so that the ion became 0.18 mol / L.
[0263] A sulfate bath was selected as the manganese plating bath. The manganese plating bath was prepared as follows: Mn 2+ Manganese sulfate was added as a soluble manganese salt so that the manganese ion became 0.92 mol / L.
[0264] The activated copper foil was connected to a power source in a way that current could be applied, and then immersed in a bismuth plating bath. Then, the current density was controlled to 2A / dm 2 , thereby electroplating bismuth on the unmasked copper foil surface in a manner to have a thickness of approximately 4 μm to produce a Bi-plated film.
[0265] Next, the copper foil with the Bi-plated film was connected to a power source in a manner that current could be applied as in the case of bismuth electroplating, and then immersed in a manganese plating bath. Thereafter, the current density was controlled to 2 A / dm 2 , thereby electroplating manganese on the unmasked copper foil surface in a manner to have a thickness of approximately 1 μm to form a Mn film.
[0266] In addition, in the step of immersing the copper foil in the plating bath, masking was performed on the surface other than the plated surface.
[0267] After electroplating, the copper foil was recovered from the plating bath, removed from the mask, cleaned with pure water and dried. Thereafter, the copper foil and the plating layers (i.e., the Bi plating film and the Mn plating film) formed on the copper foil were heat treated at 200° C. for 100 hours in an electric furnace with an argon atmosphere.
[0268] It should be noted that the heat-treated plating layer corresponds to the active material layer of the first electrode. The structure of the heat-treated plating layer, that is, the active material layer, was analyzed by surface X-ray diffraction measurement. The method of X-ray diffraction measurement is the same as that of Example 1. Figure 7 The graphs show X-ray diffraction patterns of the active material layer of the first electrode in the battery of Example 4 at the initial stage, after charge, and after charge and discharge. Figure 7 In the X-ray diffraction pattern of the initial active material layer, the X-ray diffraction pattern is indicated as "Initial". The X-ray diffraction pattern confirms that Bi4Cu4Mn3 with a cubic crystal structure and a space group belonging to Fm-3m is generated in the active material layer. It should be noted that the phase of the Cu foil as the collector is also confirmed in the X-ray diffraction pattern.
[0269] Then, the sheet was punched out into a size of 2×2 cm to obtain a first electrode. That is, the first electrode of Example 1 had a structure in which an active material layer composed of Bi4Cu4Mn3 was provided on a current collector composed of copper foil.
[0270] <Battery production>
[0271] A battery as a test cell of Example 4 was prepared in the same manner as in Example 1 except that the first electrode of Example 4 was used as the working electrode.
[0272] <Charge and discharge test>
[0273] The battery produced as the test cell was subjected to a charge and discharge test. The charge and discharge test was conducted in the same manner as the charge and discharge test of Example 1. Figure 8 : is a graph showing the results of the charge and discharge test of the battery of Example 4. Figure 8 As shown, in Example 4, the charge reaction potential changes from 0.2 to 0.6 V (vs. Li), and the discharge reaction potential becomes approximately 0.85 V (vs. Li).
[0274] <Structural changes of active materials based on X-ray diffraction>
[0275] For the first electrode charged and discharged in the same procedure as the charge and discharge test conditions in the above-mentioned "charge and discharge test", after charging and after charging and discharging, X-ray diffraction measurement is performed on the surface where the active material layer is formed. The X-ray diffraction measurement of the active material layer after charging and charging and discharging is performed in the same manner as the X-ray diffraction measurement performed on the above-mentioned initial active material layer. Figure 7 In the X-ray diffraction pattern of the active material layer after charge is the X-ray diffraction pattern indicated as "charge", and the X-ray diffraction pattern of the active material layer after charge-discharge is the X-ray diffraction pattern indicated as "charge-discharge". Figure 7 The X-ray diffraction pattern shown can confirm that Bi4Cu4Mn3 forms Li3Bi by charging and forms Bi4Cu4Mn3 again by discharging.
[0276] (Example 5)
[0277] <Fabrication of First Electrode>
[0278] The first electrode was manufactured in the same manner as in Example 4 except that the final size of the first electrode was different. In Example 5, the first electrode was punched into size.
[0279] <Solid Electrolyte>
[0280] As a solid electrolyte constituting the electrolyte layer, a sulfide solid electrolyte Li6PS5Cl (produced by Ampcera, 80 mg) was used.
[0281] <Battery production>
[0282] The obtained first electrode is arranged in an insulating outer cylinder having an inner diameter of 9.4 mm. On the active material layer of the first electrode, a solid electrolyte Li6PS5Cl (80 mg) is stacked, and then an indium-lithium alloy (molar ratio: In:Li=1:1) (200 mg) is stacked as the second electrode to obtain a stack. The indium-lithium alloy is made as follows: a small piece of lithium foil is crimped on the indium foil to diffuse lithium into the indium. For the above-mentioned stack, a pressure of 360 MPa is applied in the stacking direction to form a battery as a test battery cell having a first electrode, a solid electrolyte layer and a second electrode. In the battery as a test battery cell, the thickness of the first electrode is 1.5 μm, the thickness of the solid electrolyte layer is 500 μm, and the thickness of the second electrode is 15 μm.
[0283] Next, a current collector made of stainless steel was attached to the first electrode and the second electrode, and a current collecting lead was attached to the current collector.
[0284] Finally, an insulating nozzle is used to block the inside of the insulating outer cylinder from the external gas atmosphere, thereby hermetically sealing the inside of the cylinder.
[0285] As described above, a battery as a test battery cell of Example 5 was obtained, in which the first electrode having an active material layer formed of Bi4Cu4Mn3 was used as a working electrode and a lithium-indium alloy was used as a counter electrode.
[0286] <Charge and discharge test>
[0287] In the same manner as in Example 2, a charge and discharge test of the fabricated battery was performed. Fig. 9 : is a graph showing the results of the charge and discharge test of the battery of Example 5. Fig. 9When the InLi-based potential shown is converted to the Li-based potential, the charge reaction potential of the first cycle changes from 0.32 to 0.6 V (vs. Li) in Example 5, which has a large slope. However, the charge reaction potential of the second cycle and thereafter changes from 0.5 to 0.7 V (vs. Li), and the discharge reaction potential becomes around 0.85 V (vs. Li).
[0288] (Example 6)
[0289] <Fabrication of First Electrode>
[0290] The first electrode was manufactured in the same manner as in Example 4 except that the final size of the first electrode was different. In Example 6, the first electrode was punched into size.
[0291] <Production of solid electrolyte>
[0292] In the same manner as in Example 3, a solid electrolyte having a composition of Li3YBr4Cl2 was prepared.
[0293] <Battery production>
[0294] A battery serving as a test cell of Example 6 was produced in the same manner as in Example 5, except that Li3YBr4Cl2 (80 mg) was used in place of the solid electrolyte Li6PS5Cl (80 mg) in the production of the solid electrolyte layer.
[0295] <Charge and discharge test>
[0296] The prepared battery was subjected to a charge and discharge test in the same manner as in Example 3. Fig.10 : is a graph showing the results of the charge and discharge test of the battery of Example 6. Fig.10 When the InLi-based potential shown is converted to the Li-based potential, the charge reaction potential of the first cycle changes from 0.37 to 0.75 V (vs. Li) in Example 6, which has a large slope. However, the charge reaction potential of the second cycle and thereafter changes from 0.52 to 0.75 V (vs. Li), and the discharge reaction potential becomes around 0.85 V (vs. Li).
[0297] (Reference Example 1)
[0298] <Fabrication of First Electrode>
[0299] As a pretreatment, a nickel foil (10 cm×10 cm, thickness: 12 μm) was pre-degreased with an organic solvent, and then one side was masked and immersed in an acidic solvent to degrease and activate the copper foil surface. 3+Bismuth methanesulfonate was added as a soluble bismuth salt so that the ion concentration was 0.18 mol / L to prepare a plating bath. The activated nickel foil was connected to a power source in a manner that current could be applied, and then immersed in the plating bath. Thereafter, the current density was controlled to 2 A / dm 2 , thereby electroplating bismuth on the unmasked nickel foil surface in a manner of approximately 5 μm in thickness. After electroplating, the nickel foil is recovered from the acid bath, removed from the mask, and then cleaned and dried with pure water. Thereafter, the nickel foil electroplated with bismuth is heat treated at 400°C for 60 hours in an electric furnace forming an argon atmosphere. After heat treatment, the Bi-plated layer on the nickel foil is subjected to surface X-ray diffraction measurement in the same manner as in Example 1. The X-ray diffraction pattern obtained according to the measurement confirmed that BiNi, which is a monoclinic crystal with a crystal structure belonging to the space group C2 / m, was generated. Thereafter, the laminate having a layer formed by BiNi on the nickel foil was punched out into a size of 2×2 cm to obtain a first electrode. That is, the first electrode of Reference Example 1 has a structure in which an active material layer formed by BiNi is provided on a current collector formed by a nickel foil.
[0300] <Battery production>
[0301] A battery as a test cell of Reference Example 1 was prepared in the same manner as in Example 1 except that the first electrode of Reference Example 1 was used as the working electrode.
[0302] <Charge and discharge test>
[0303] The charge and discharge test was carried out in the same manner as in Example 1 except that the test battery cell of Reference Example 1 was used. Fig.11 Graph showing the results of the charge and discharge test of the battery of Reference Example 1. Fig.11 As shown, in the battery of Reference Example 1, the charge reaction potential decreased to 0.44 to 0.5 V (vs. Li), and the discharge reaction potential became around 0.8 V (vs. Li).
[0304] (Reference Example 2)
[0305] <Fabrication of First Electrode>
[0306] The first electrode was produced in the same manner as in Reference Example 1 except that the final size of the first electrode was different. size.
[0307] <Solid Electrolyte>
[0308] As a solid electrolyte constituting the electrolyte layer, a sulfide solid electrolyte Li6PS5Cl (produced by Ampcera, 80 mg) was used.
[0309] <Battery production>
[0310] The obtained first electrode is arranged in an insulating outer cylinder having an inner diameter of 9.4 mm. On the active material layer of the first electrode, a solid electrolyte Li6PS5Cl (80 mg) is stacked, and then an indium-lithium alloy (molar ratio: In:Li=1:1) (200 mg) is stacked as the second electrode to obtain a stack. The indium-lithium alloy is made as follows: a small piece of lithium foil is crimped on the indium foil to diffuse lithium into the indium. For the above-mentioned stack, a pressure of 360 MPa is applied in the stacking direction to form a battery as a test battery cell having a first electrode, a solid electrolyte layer and a second electrode. In the battery as a test battery cell, the thickness of the first electrode is 1.5 μm, the thickness of the solid electrolyte layer is 500 μm, and the thickness of the second electrode is 15 μm.
[0311] Next, a current collector made of stainless steel was attached to the first electrode and the second electrode, and a current collecting lead was attached to the current collector.
[0312] Finally, an insulating nozzle is used to block the inside of the insulating outer cylinder from the external gas atmosphere, thereby hermetically sealing the inside of the cylinder.
[0313] As described above, a battery as a test cell of Reference Example 2 was obtained, in which the first electrode including the active material layer formed of BiNi was used as the working electrode and the lithium-indium alloy was used as the counter electrode.
[0314] <Charge and discharge test>
[0315] The battery was charged and discharged under the following conditions. The theoretical capacity of Bi was 384 mAh / g based on the weight of Bi after electroplating. The battery was charged to -0.42 V (i.e., 0.2 V (vs. Li+ / Li)) at a constant current value of 0.05 IT based on the Bi rate. The battery was then discharged to 1.38 V (i.e., 2.0 V (vs. Li+ / Li)). The battery was then charged to -0.42 V (i.e., 0.2 V (vs. Li+ / Li)). The battery was tested in a thermostatic chamber at 25°C. Fig.12 : is a graph showing the results of the charge and discharge test of the battery of Reference Example 2. Fig.12 When the InLi-based potential shown is converted to the Li-based potential, in Reference Example 2, the charge reaction potential changes from 0.48 to 0.53 V (vs. Li), and the discharge reaction potential becomes approximately 0.8 V (vs. Li).
[0316] (Reference Example 3)
[0317] <Fabrication of First Electrode>
[0318] The first electrode was produced in the same manner as in Reference Example 1 except that the final size of the first electrode was different. size.
[0319] <Production of solid electrolyte>
[0320] In the same manner as in Example 3, a solid electrolyte having a composition of Li3YBr4Cl2 was prepared.
[0321] <Battery production>
[0322] A battery as a test battery cell of Reference Example 3 was produced in the same manner as Reference Example 2, except that Li3YBr4Cl2 (80 mg) was used instead of the solid electrolyte Li6PS5Cl (80 mg) in the production of the solid electrolyte layer.
[0323] <Charge and discharge test>
[0324] The prepared battery was subjected to a charge and discharge test in the same manner as in Reference Example 2. Fig.13 : is a graph showing the results of the charge and discharge test of the battery of Reference Example 3. Fig.13 When the InLi-based potential shown is converted to the Li-based potential, in Reference Example 3, the charge reaction potential after the first cycle changes from 0.38 to 0.76 V (vs. Li), and the discharge reaction potential becomes approximately 0.82 V (vs. Li).
[0325] From the above results, a battery having a first electrode having an active material layer containing an alloy containing Bi and Mn has improved energy efficiency compared to a battery having a first electrode having an active material layer formed of BiNi and not containing an alloy containing Bi and Mn.
[0326] It should be noted that in the embodiments described in this specification, the halide solid electrolyte Li3YBr4Cl2 and the sulfide solid electrolyte Li6PS5Cl are used as solid electrolytes, but it can be expected that the same effect can be obtained even with other general solid electrolytes.
[0327] Industrial Applicability
[0328] The battery disclosed herein can be used as, for example, an all-solid lithium secondary battery or the like.
Claims
1. A battery comprising: The first electrode, the second electrode, and an electrolyte layer located between the first electrode and the second electrode, The first electrode has: Current collector, and an active material layer located between the current collector and the electrolyte layer, The active material layer contains an alloy including Bi and Mn.
2. The battery according to claim 1, in, The active material layer includes a material selected from LiBi and Li 3 At least one of the group consisting of Bi.
3. The battery according to claim 1 or 2, in, The active material layer contains BiMn as an active material.
4. The battery according to claim 3, in, The BiMn has a crystal structure belonging to a space group of P63 / mmc.
5. The battery according to any one of claims 1 to 4, in, The active material layer contains Bi 4 Cu 4 Mn 3 As active substance.
6. The battery according to claim 5, in, The Bi 4 Cu 4 Mn 3 The crystal structure has a space group assigned to Fm-3m.
7. The battery according to any one of claims 1 to 6, in, The active material layer does not contain a solid electrolyte.
8. The battery according to any one of claims 1 to 7, in, The current collector includes Cu.
9. The battery according to any one of claims 1 to 8, in, The active material layer is a heat-treated plating layer.
10. The battery according to any one of claims 1 to 9, in, The electrolyte layer contains an electrolyte solution.
11. The battery according to claim 10, in, The electrolyte contains vinylene carbonate as a solvent.
12. The battery according to any one of claims 1 to 9, in, The electrolyte layer is a solid electrolyte layer.
13. The battery according to claim 12, in, The solid electrolyte layer includes a halide solid electrolyte, The halide solid electrolyte does not contain sulfur.
14. The battery according to claim 12, in, The solid electrolyte layer includes a sulfide solid electrolyte.
15. The battery according to any one of claims 1 to 14, in, The first electrode is a negative electrode, The second electrode is a positive electrode.
16. A method for manufacturing an electrode, comprising the following steps: The step of forming a coating layer including a Bi coating film and a Mn coating film on a current collector by electroplating; and, The step of heating the current collector and the plating layer to obtain an electrode having an active material layer formed on the current collector, wherein the active material layer contains an alloy containing Bi and Mn.
17. The method for manufacturing an electrode according to claim 16, in, The current collector includes Cu.