Container and method for producing a container
Through die-casting liquid forging composite process and anodizing treatment, the problems of blistering and internal pores on the surface of die-casting cooking vessels are solved, and high-quality container matrix and anodized film are realized, which improves yield and user experience.
Patent Information
- Application Number
- CN202310553739.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-12
AI Technical Summary
The existing cooking utensils have problems such as blistering on the surface, internal air holes or shrinkage through die-casting molding process, resulting in high defect rate and poor user experience, and poor anodized film effect.
By adopting die-casting liquid forging composite process, local extrusion is performed after the metal melt is cooled into semi-solid parts, combined with the liquid die forging process, the filling speed is dynamically adjusted to reduce the air rolling and cooling shrinkage, forming a high-quality container matrix, and A continuously dense anodized film is prepared on its surface.
It significantly reduces the pore rate of the product and the risk of coating foaming, improves the yield rate and user experience, and ensures the continuity and advanced texture of the anodized film, improving the competitiveness of the product.
Smart Images

Figure CN118924102A_ABST
Abstract
Description
[0001] This application claims the priority of the Chinese patent application filed with the State Intellectual Property Office of China on May 9, 2023, with application number "2023105152141" and invention name "Container and Method for Preparing Container", the entire contents of which are incorporated by reference in this application. Technical Field
[0002] The invention relates to the field of cooking appliances, and in particular to a container and a method for preparing the container. Background Art
[0003] As people's living standards continue to improve, the requirements for cooking utensils on the market are becoming more refined and stringent. In order to achieve good non-stick properties, the inside of cooking utensils requires a high-quality non-stick coating. The outside of cooking utensils must not only be rust-proof and wear-resistant but also have a high-grade texture and recognition. Anodizing treatment can achieve such effects on the outer surface.
[0004] Cooking utensils have always been produced by die-casting. During the die-casting process, the metal crystallizes quickly and there is air entrainment during the metal liquid filling process. Therefore, the surface of the die-cast cooking utensils is prone to blistering and the inside is prone to pores or shrinkage holes, which significantly affects the product quality. Especially after the non-stick coating is processed on the inner surface, when the die-cast cooking utensils are heated, the gas remaining in the internal pores will overflow, and the non-stick coating is very likely to bubble or even partially fall off. This not only causes a high product defect rate, but also after the die-cast cooking utensils enter the market, there is still a risk that the internal gas will break the non-stick coating of the utensils after multiple cooking and heating, which greatly affects the user experience.
[0005] Therefore, how to propose a preparation method that can ensure the casting performance of die-cast cooking utensils during die-casting, make the product easy to demold during the die-casting process, be suitable for die-casting production, and can easily prepare a qualified oxide film on the surface of the die-cast cooking utensils has become a problem that needs to be solved urgently. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0007] To this end, a first object of the present invention is to provide a container.
[0008] The second object of the present invention is to provide a method for preparing a container.
[0009] In view of this, the technical solution of the first aspect of the present invention provides a container, including: a container base, which is prepared by a die-casting and liquid forging composite process; and an anodized film located on the outer surface of the container base.
[0010] According to the container provided by the present invention, it includes a container base and an anodic oxide film arranged on the outer surface of the container base. Among them, the container base has a cavity for accommodating items, which constitutes the main structure of the container and can meet the basic needs of holding items. Of course, in addition to the container base, the container can also include a coating arranged on the inner and outer surfaces of the container base, such as a non-stick coating arranged in the container base, or a protective coating arranged outside the container base. When the container base is formed, the container base is prepared by a die-casting liquid forging composite process.
[0011] Specifically, the preparation steps are as follows: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity under high pressure. Specifically, the molten metal is filled into the mold cavity in the same way as the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity and the molten metal can be quickly cooled in the mold cavity. After the molten metal is filled, the molten metal will gradually cool in the cavity, and when the molten metal is cooled into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is extruded until the semi-solid part is formed into a container matrix. In this method, after the molten metal is cooled into a semi-solid part, the semi-solid part is locally extruded until the end, and this method is similar to the liquid die forging process, which greatly solves the problems of many pores, non-density and high scrap rate of parts formed by the die casting process. That is, in the process of preparing the container matrix of this application, the first half step adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), so that the two processes of die casting and liquid die forging are combined together, that is, a new process is provided, that is, the die casting liquid forging composite process. This process, through targeted transformation of the die casting technology, injects the function of liquid die forging, and reduces the air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate the shrinkage of the semi-solid casting when the metal cools and shrinks, thereby greatly reducing the product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking containers, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield and quality of the prepared container matrix and reducing its preparation cost.
[0012] In addition, since the container matrix is prepared by the die-casting liquid forging composite process, its surface quality is high, which is specifically reflected in that the casting surface is not easy to bubble, and pores or shrinkage holes are not easy to be generated inside. Therefore, when the anodized film is set on its surface, it is relatively easy to obtain a qualified oxide film, that is, the prepared oxide film is relatively continuous, dense, and has a good coloring effect. In the existing scheme, since the container matrix is mostly produced by die-casting, its surface quality is not high, so the effect of the anodized film formed on the surface is not good, which is specifically manifested in that the oxide film is discontinuous and not dense, and the oxidation coloring effect is poor. The present application can prepare a complete and continuous oxidation mold with good coloring effect by changing the process of the container matrix. In this way, the appearance of containers such as pots and pans after production is ensured, so that the prepared containers such as pots and pans have high-grade texture and recognition, thereby improving the competitiveness of the product and improving the user experience.
[0013] Furthermore, the container further includes a non-stick coating. The non-stick coating is located on the inner wall of the container substrate. The non-stick property of the container is ensured by providing the non-stick coating. Specifically, the non-stick coating may be any one of a PTFE (Polytetrafluoroethylene, Teflon) coating, a PFA (Polyfluoroalkoxy, soluble polytetrafluoroethylene) coating, a PEEK (Polyetheretherketone, polyetheretherketone) coating, and a ceramic coating.
[0014] In the above technical solution, the weight percentage of Si in the container matrix is greater than or equal to 0 and less than or equal to 0.5%, that is, the container matrix is made of a low-silicon alloy.
[0015] In this technical solution, the melt used to prepare the container matrix contains silicon, and the weight percentage of silicon is less than 0.5%. Because, in order to pursue good formability, die-casting products often use die-cast aluminum with a high silicon content, and the presence of silicon can improve the fluidity of cast aluminum. However, if the silicon content is too high, it will be difficult to obtain a qualified oxide film on the surface of the die-cast aluminum, which is specifically manifested as discontinuous and non-dense oxide film and poor oxidation coloring effect. If non-aluminum-silicon alloys are used, the casting performance during die-casting will be extremely poor, not only will the shrinkage tendency be large, but it will also be difficult to demold, and it is not suitable for die-casting production at all. Therefore, in the process of preparing the container matrix, the present application selects a material containing silicon, that is, the material itself may contain silicon impurity elements, and the silicon element cannot be completely eliminated during smelting. Under normal circumstances, the silicon content in the smelted material is relatively high, and the present application deliberately controls the weight percentage of silicon to within 0.5%, thereby not only ensuring the fluidity of cast aluminum, overcoming the shortcoming that non-aluminum-silicon alloys have poor fluidity and are not suitable for die-casting production, but also using low-silicon content aluminum alloys to manufacture the container matrix, so that a uniform and continuous anodized film can be formed on its outer surface, thereby improving the protection effect and surface texture of the prepared product.
[0016] In the above technical solution, the container substrate includes an aluminum-silicon alloy substrate, because the aluminum-silicon alloy has high fluidity and good thermal conductivity, thereby ensuring the surface quality of the prepared container substrate, the thermal conductivity of the container substrate, and the heating efficiency.
[0017] Furthermore, the container base is generally made of a material with a thermal conductivity greater than or equal to 90 W / m·k and less than or equal to 110 W / m·k, so that the thermal conductivity and heat storage effect are relatively moderate. If the thermal conductivity is too high, it will lead to poor heat storage effect.
[0018] Furthermore, the thickness of the anodized film is greater than or equal to 10 μm and less than or equal to 50 μm.
[0019] Furthermore, the wall thickness of the container base is greater than or equal to 2 mm and less than or equal to 12 mm.
[0020] In the above technical solution, the diameter of the holes in the container matrix is less than or equal to 1.5 mm, and the porosity of the preset holes in the container matrix is greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container matrix is formed, the number of holes in the unit area of 10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container matrix is greater than or equal to twice the diameter of each preset hole itself. This type of container matrix makes the bubbles relatively small, the interior of the parts is denser, and ensures the qualified rate of the product.
[0021] The technical solution of the second aspect of the present invention provides a method for preparing a container, which is used to prepare the container provided by any technical solution of the first aspect. The preparation method comprises: filling molten metal into a mold cavity of a mold at a preset filling speed; when the molten metal in the mold cavity of the mold is formed into a semi-formed part, a preset part of the semi-formed part is squeezed until the molten metal in the mold cavity is formed into a container matrix; after the container matrix is taken out of the mold, anodizing the outer surface of the container matrix to form an anodized film that meets preset requirements on the outer surface of the container matrix.
[0022] According to the preparation method of the container provided by the present invention, when the container matrix is formed, the container matrix is prepared and formed by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity by high pressure. Specifically, the molten metal is filled into the mold cavity in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly cooled in the mold cavity. After the molten metal is filled, the molten metal will gradually cool in the cavity, and when the molten metal is cooled into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is extruded until the semi-solid part is formed into the container matrix. In this method, after the molten metal is cooled into a semi-solid part, the semi-solid part is locally extruded until the end, and this method is similar to the liquid die forging process, which greatly solves the problems of many pores, non-density and high scrap rate of parts formed by the die casting process. That is, in the process of preparing the container matrix of this application, the first half step adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), so that the two processes of die casting and liquid die forging are combined together, that is, a new process is provided, that is, the die casting liquid forging composite process. This process, through targeted transformation of the die casting technology, injects the function of liquid die forging, and reduces the air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate the shrinkage of the semi-solid casting when the metal cools and shrinks, thereby greatly reducing the product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking containers, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield and quality of the prepared container matrix and reducing its preparation cost.
[0023] In addition, since the container matrix is prepared by the die-casting liquid forging composite process, its surface quality is high, which is specifically reflected in that the casting surface is not easy to bubble, and pores or shrinkage holes are not easy to be generated inside. Therefore, when the anodized film is set on its surface, it is relatively easy to obtain a qualified oxide film, that is, the prepared oxide film is relatively continuous, dense, and has a good coloring effect. In the existing scheme, since the container matrix is mostly produced by die-casting, its surface quality is not high, so the effect of the anodized film formed on the surface is not good, which is specifically manifested as the oxide film is discontinuous and not dense, and the oxidation coloring effect is poor. However, by changing the process of the container matrix, the present application can prepare a complete and continuous oxidation mold with good coloring effect when the anodized film is prepared on its surface later. In this way, the appearance of the container and other containers after production is ensured, so that the prepared containers and other containers have high-grade texture and recognition, thereby improving the competitiveness of the product and improving the user experience.
[0024] In the above technical solution, in the step of filling the molten metal into the cavity of the mold at a preset filling speed, the injection pressure is greater than or equal to 65 MPa and less than or equal to 110 MPa.
[0025] Furthermore, the injection speed is greater than or equal to 5 m / s and less than or equal to 8 m / s.
[0026] Furthermore, the filling time of the molten metal is greater than or equal to 0.02 s and less than or equal to 0.05 s.
[0027] Furthermore, the filling speed of the molten metal is greater than 0 and less than or equal to 0.8 m / s.
[0028] In this technical solution, when the molten metal is filled into the mold cavity, it is necessary to dynamically adjust the filling speed to control the filling time according to the actual situation, so as to fully control the filling process of the molten metal, and avoid the filling speed being too fast or too slow, which may cause the parts to fail to cool as required, so as to ensure the quality of the parts after molding, and further reduce the bubbles in the parts, making the parts more dense. By reasonably controlling the specific pressure, injection speed and filling time, high-speed filling of the molten metal can be achieved, so that the molten metal can be cooled quickly. At the same time, by dynamically adjusting the filling speed, air entrainment can be reduced, and the holes in the product after the product is molded can be reduced.
[0029] In the above technical solution, when the preset part of the semi-formed part is extruded, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s. This solution can eliminate the shrinkage holes formed by cooling shrinkage by applying the extrusion force of the above parameters, and obtain high-strength parts with fine and uniform grains and dense structure, so as to ensure the quality of the parts after forming, and solve the problem of many pores and high scrap rate of die castings.
[0030] In the above technical solution, the molten metal includes a cast aluminum alloy molten metal, and the weight percentage of Si in the cast aluminum alloy molten metal is greater than or equal to 0 and less than or equal to 0.5%.
[0031] In this technical solution, the melt for preparing the container matrix contains silicon, and the weight percentage of silicon is less than 0.5%. Because, in order to pursue good formability, die-casting products often use die-cast aluminum with a high silicon content, and the presence of silicon can improve the fluidity of cast aluminum. However, if the silicon content is too much, it will be difficult to obtain a qualified oxide film on the surface of the die-cast aluminum, which is specifically manifested as discontinuous and non-dense oxide films, and poor oxidation coloring effects. If non-aluminum-silicon alloys are used, the casting performance during die-casting will be extremely poor, not only with a large shrinkage tendency, but also with difficulty in demolding, and it is not suitable for die-casting production at all. Therefore, in the process of preparing the container matrix, the present application selects a material containing silicon, and controls the weight percentage of silicon within 0.5%, thereby not only ensuring the fluidity of cast aluminum, but also overcoming the shortcoming that non-aluminum-silicon alloys have poor fluidity and are not suitable for die-casting production. At the same time, the container matrix is manufactured using a low-silicon aluminum alloy, so that a uniform and continuous anodized film can be formed on its outer surface, thereby improving the protection effect and surface texture of the prepared product.
[0032] In the above technical solution, the preparation method of the container also includes demolding pretreatment. The demolding pretreatment specifically includes opening the mold, taking out the container matrix and cooling it after the molten metal in the cavity is formed into the container matrix, and processing the cooled container matrix to a preset size and / or preset accuracy. When the container matrix is processed by the die-casting liquid forging composite process, some processing allowances are generally reserved for the container matrix. Therefore, after the container is basically prepared and formed, the container matrix can be processed into the size and accuracy required by the drawing (such as roughness, flatness and coaxiality, etc.) by machining and other methods.
[0033] In the above technical solution, the preparation method of the container also includes roughness treatment. The roughness treatment specifically includes: after the container substrate is taken out from the mold, the inner and outer surfaces of the container substrate are subjected to roughness treatment until the roughness Ra of the inner and outer surfaces of the container substrate is greater than or equal to 2μm and less than or equal to 5μm. Furthermore, this step is generally performed after the demolding pretreatment. If there is no demolding pretreatment step, the roughness treatment can be performed directly after the part is demolded. By performing roughness treatment on the container substrate, the surface quality of the container substrate can be guaranteed, and preparations can be made for subsequent coating spraying on the container substrate.
[0034] Further, the roughening treatment includes sandblasting and / or grinding.
[0035] Furthermore, the preparation method of the container also includes forming a non-stick coating. The step of forming the non-stick coating specifically includes: forming a non-stick coating on the inner wall surface of the container substrate. The non-stick performance of the inner wall surface of the container can be improved by providing the non-stick coating. The non-stick coating can specifically include one or more of PTFE coating, PFA coating, PEEK coating, and ceramic coating. Furthermore, after the roughness treatment, the non-stick coating is formed on the inner wall surface of the container substrate, that is, the roughness treatment is performed first, and then the non-stick coating is formed.
[0036] Furthermore, the preparation method also includes degreasing the container substrate after the step of roughening and before the step of forming the non-stick coating. After the prepared container substrate is processed by machining or roughening, there will be some grease on the surface, so degreasing is required before forming the non-stick coating. The degreasing treatment can be high-temperature heating. At this time, the container can be heated. The specific heating temperature can be 350°C-420°C, and the heating temperature can last for 8min-15min. Of course, the degreasing treatment can also be carried out by other methods such as chemical degreasing.
[0037] In the above technical solution, the step of roughness treatment and the step of processing the cooled container base to a preset size and / or a preset precision are located before the step of anodizing the outer surface of the container base. That is, the steps of roughness treatment and demoulding pretreatment are performed first, and the anodizing treatment is performed last, because the anodizing treatment is to form a high-quality film layer on the surface, and this step is performed last, which can prevent the anodized film from being scratched or damaged due to the preparation of the non-stick coating, etc. after the preparation is completed.
[0038] In the above technical solution, the diameter of the holes in the container matrix is less than or equal to 1.5 mm, and the porosity of the preset holes in the container matrix is greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container matrix is formed, the number of holes in the unit area of 10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container matrix is greater than or equal to twice the diameter of each preset hole itself. This type of container matrix makes the bubbles relatively small, the interior of the parts is denser, and ensures the qualified rate of the product.
[0039] In a specific preparation method, the preparation process is as follows: after the molten metal in the cavity is formed into a container matrix, the mold is opened, the container matrix is taken out and cooled, and the cooled container matrix is processed to a preset size and / or preset accuracy; then degreasing treatment is performed, followed by sandblasting and other roughness treatments, and then a non-stick coating treatment is performed, and finally anodizing treatment is performed.
[0040] Additional aspects and advantages of the present invention will become apparent from the following description or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0042] Figure 1 A schematic structural diagram of a container according to an embodiment of the present invention is shown;
[0043] Figure 2 A microscopic structure diagram of a container according to an embodiment of the present invention is shown;
[0044] Figure 3 A schematic flow chart of a method for preparing a container according to an embodiment of the present invention is shown;
[0045] Figure 4 A schematic flow chart of a method for preparing a container according to another embodiment of the present invention is shown.
[0046] in, Figure 1 and Figure 2 The corresponding relationship between the reference numerals and the component names is as follows:
[0047] 1 container, 12 container base, 14 anodized film, 16 non-stick coating. DETAILED DESCRIPTION
[0048] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0049] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0050] Refer to the following Figures 1 to 4 The container 1 and the preparation method thereof provided by the present invention are described.
[0051] like Figure 1 and Figure 2 As shown, the technical solution of the first aspect of the present invention provides a container 1, comprising a container substrate 12 and an anodic oxide film 14. The weight percentage of Si in the container substrate 12 is greater than 0 and less than or equal to 0.5%. The anodic oxide film 14 is located on the outer surface of the container substrate 12.
[0052] According to the container 1 provided by the present invention, it includes a container base 12 and an anodized film 14 arranged on the outer surface of the container base 12. Among them, the container base 12 has a cavity for accommodating articles, which constitutes the main structure of the container 1 and can meet the basic needs of holding articles. Of course, in addition to the container base 12, the container 1 can also include a coating arranged on the inner and outer surfaces of the container base 12, such as a non-stick coating 16 arranged in the container base 12, or a protective coating arranged outside the container base 12. When the container base 12 is formed, the container base 12 is prepared by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity of the mold through high pressure. Specifically, the molten metal is filled into the mold cavity of the mold in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly cooled in the mold cavity. After the molten metal is filled, the molten metal will gradually cool in the cavity, and when the molten metal is cooled into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is extruded until the semi-solid part is formed into the container matrix 12. In this way, after the molten metal is cooled into a semi-solid part, the semi-solid part is locally extruded until the end, and this method is similar to the liquid die forging process, which greatly solves the problems of many pores, non-density and high scrap rate of parts formed by the die casting process. That is, in the process of preparing the container matrix 12, the first half of the step of the present application adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), thereby combining the two processes of die casting and liquid die forging together, that is, providing a new process, that is, the die casting and liquid forging composite process. This process, through targeted transformation of die casting technology, injects the function of liquid die forging, reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the die to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal cools and shrinks, thereby greatly reducing product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the cooking container 1 is manufactured by creatively utilizing the die casting-liquid die forging composite process, thereby improving the yield rate of the original die casting aluminum alloy, improving the cost performance, and then ensuring the yield rate and quality of the prepared container matrix 12, and reducing its preparation cost.
[0053] In addition, since the container base 12 is prepared by the die-casting liquid forging composite process, its surface quality is high, which is specifically reflected in that the casting surface is not easy to bubble, and pores or shrinkage holes are not easy to be generated inside, so that when the anodized film 14 is set on its surface, it is relatively easy to obtain a qualified oxide film, that is, the prepared oxide film is relatively continuous, dense, and has a good coloring effect. In the existing scheme, since the container base 12 is mostly produced by die-casting, its surface quality is not high, so that the effect of the anodized film 14 formed on the surface is not good, which is specifically manifested as the oxide film is discontinuous and not dense, and the oxidation coloring effect is poor. However, the present application can prepare a complete and continuous oxidation mold with good coloring effect by changing the process of the container base 12. In this way, the appearance of the container 1 such as pots and pans after production is completed is ensured, so that the prepared container 1 such as pots and pans has a high-grade texture and recognition, thereby improving the competitiveness of the product and improving the user experience.
[0054] Furthermore, if Figure 1 and Figure 2 As shown, the container 1 further includes a non-stick coating 16. The non-stick coating 16 is located on the inner wall of the container substrate 12. The non-stick property of the container 1 is ensured by providing the non-stick coating 16. Specifically, the non-stick coating 16 can be any one of a PTFE coating, a PFA coating, a PEEK coating, and a ceramic coating.
[0055] In the above technical solution, the weight percentage of Si in the container base 12 is greater than or equal to 0 and less than or equal to 0.5%, that is, the container base 12 is made of a low-silicon alloy.
[0056] In this technical solution, the melt for preparing the container matrix 12 contains silicon, and the weight percentage of silicon is less than 0.5%. Because, in order to pursue good formability, die-casting products often use die-cast aluminum with a high silicon content, and the presence of silicon can improve the fluidity of cast aluminum. However, if the silicon content is too much, it will be difficult to obtain a qualified oxide film on the surface of the die-cast aluminum, which is specifically manifested as discontinuous and non-dense oxide films, and poor oxidation coloring effects. If non-aluminum-silicon alloys are selected, the casting performance during die-casting will be extremely poor, not only with a large shrinkage tendency, but also difficult to demold, and not suitable for die-casting production at all. Therefore, in the process of preparing the container matrix 12, the present application selects a material containing silicon elements, and controls the weight percentage of silicon within 0.5%, thereby not only ensuring the fluidity of cast aluminum, but also overcoming the shortcoming that non-aluminum-silicon alloys have poor fluidity and are not suitable for die-casting production. At the same time, the container matrix 12 is manufactured using a low-silicon aluminum alloy, so that a uniform and continuous anodized film 14 can be formed on its outer surface, thereby improving the protection effect and surface texture of the prepared product.
[0057] In the above technical solution, the container substrate 12 includes an aluminum silicon alloy substrate, because the aluminum silicon alloy has high fluidity and good thermal conductivity, thereby ensuring the surface quality of the prepared container substrate 12, ensuring the thermal conductivity of the container substrate 12, and ensuring the heating efficiency.
[0058] Furthermore, the container base 12 is generally made of a material with a thermal conductivity of less than 110 W / m·k, so that the thermal conductivity and the heat storage effect are relatively moderate. If the thermal conductivity is too high, the heat storage effect will be poor.
[0059] Furthermore, the thickness of the anodized film 14 is greater than or equal to 10 μm and less than or equal to 50 μm.
[0060] Furthermore, the wall thickness of the container base 12 is greater than or equal to 2 mm and less than or equal to 12 mm.
[0061] In the above technical solution, the diameter of the hole in the container matrix 12 is less than or equal to 1.5 mm, and the porosity of the preset holes in the container matrix 12 is greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container matrix 12 is formed, the number of holes in the unit area of 10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container matrix 12 is greater than or equal to twice the diameter of each preset hole itself. This type of container matrix 12 makes the bubbles less, the interior of the parts is denser, and ensures the qualified rate of the product.
[0062] like Figure 3 As shown, the technical solution of the second aspect of the present invention provides a method for preparing a container, which is used to prepare the container provided by any technical solution of the first aspect (such as Figure 1 and Figure 2 The preparation method comprises:
[0063] S302, filling the molten metal into the mold cavity at a preset filling speed.
[0064] S304, when the molten metal in the mold cavity is formed into a semi-formed part, a preset portion of the semi-formed part is extruded until the molten metal in the cavity is formed into a container base.
[0065] S306, after the container substrate is taken out from the mold, an anodizing treatment is performed on the outer surface of the container substrate to form an anodized film that meets preset requirements on the outer surface of the container substrate.
[0066] According to the preparation method of the container provided by the present invention, when the container matrix is formed, the container matrix is prepared and formed by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity by high pressure. Specifically, the molten metal is filled into the mold cavity in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly cooled in the mold cavity. After the molten metal is filled, the molten metal will gradually cool in the cavity, and when the molten metal solidifies into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is extruded until the semi-solid part is formed into the container matrix. In this method, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally extruded until the end, and this method is similar to the liquid die forging process, which greatly solves the problem of many pores, non-density and high scrap rate of parts formed by the die casting process. That is, in the process of preparing the container matrix of this application, the first half step adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), so that the two processes of die casting and liquid die forging are combined together, that is, a new process is provided, that is, the die casting liquid forging composite process. This process, through targeted transformation of the die casting technology, injects the function of liquid die forging, reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing the product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking containers, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield and quality of the prepared container matrix and reducing its preparation cost.
[0067] In addition, since the container matrix is prepared by the die-casting liquid forging composite process, its surface quality is high, which is specifically reflected in that the casting surface is not easy to bubble, and pores or shrinkage holes are not easy to be generated inside. Therefore, when the anodized film is set on its surface, it is relatively easy to obtain a qualified oxide film, that is, the prepared oxide film is relatively continuous, dense, and has a good coloring effect. In the existing scheme, since the container matrix is mostly produced by die-casting, its surface quality is not high, so the effect of the anodized film formed on the surface is not good, which is specifically manifested as the oxide film is discontinuous and not dense, and the oxidation coloring effect is poor. However, by changing the process of the container matrix, the present application can prepare a complete and continuous oxidation mold with good coloring effect when the anodized film is prepared on its surface later. In this way, the appearance of the container and other containers after production is ensured, so that the prepared containers and other containers have high-grade texture and recognition, thereby improving the competitiveness of the product and improving the user experience.
[0068] In the above technical solution, in the step of filling the molten metal into the cavity of the mold at a preset filling speed, the injection pressure is greater than or equal to 65 MPa and less than or equal to 110 MPa.
[0069] Furthermore, the injection speed is greater than or equal to 5 m / s and less than or equal to 8 m / s.
[0070] Furthermore, the filling time of the molten metal is greater than or equal to 0.02 s and less than or equal to 0.05 s.
[0071] Furthermore, the filling speed of the molten metal is greater than 0 and less than or equal to 0.8 m / s.
[0072] In this technical solution, when the molten metal is filled into the mold cavity, it is necessary to dynamically adjust the filling speed to control the filling time according to the actual situation, so as to fully control the filling process of the molten metal, and avoid the filling speed being too fast or too slow, which may cause the parts to fail to cool as required, so as to ensure the quality of the parts after molding, and further reduce the bubbles in the parts, making the parts more dense. By reasonably controlling the specific pressure, injection speed and filling time, high-speed filling of the molten metal can be achieved, so that the molten metal can be cooled quickly. At the same time, by dynamically adjusting the filling speed, air entrainment can be reduced, and the holes in the product after the product is molded can be reduced.
[0073] In the above technical solution, when the preset part of the semi-formed part is extruded, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s. This solution can eliminate the shrinkage holes formed by cooling shrinkage by applying the extrusion force of the above parameters, and obtain high-strength parts with fine and uniform grains and dense structure, so as to ensure the quality of the parts after forming, and solve the problem of many pores and high scrap rate of die castings.
[0074] In the above technical solution, the molten metal includes a cast aluminum alloy molten metal, and the weight percentage of Si in the cast aluminum alloy molten metal is greater than 0 and less than or equal to 0.5%.
[0075] In this technical solution, the melt for preparing the container matrix contains silicon, and the weight percentage of silicon is less than 0.5%. Because, in order to pursue good formability, die-casting products often use die-cast aluminum with a high silicon content, and the presence of silicon can improve the fluidity of cast aluminum. However, if the silicon content is too much, it will be difficult to obtain a qualified oxide film on the surface of the die-cast aluminum, which is specifically manifested as discontinuous and non-dense oxide films, and poor oxidation coloring effects. If non-aluminum-silicon alloys are used, the casting performance during die-casting will be extremely poor, not only with a large shrinkage tendency, but also with difficulty in demolding, and it is not suitable for die-casting production at all. Therefore, in the process of preparing the container matrix, the present application selects a material containing silicon, and controls the weight percentage of silicon within 0.5%, thereby not only ensuring the fluidity of cast aluminum, but also overcoming the shortcoming that non-aluminum-silicon alloys have poor fluidity and are not suitable for die-casting production. At the same time, the container matrix is manufactured using a low-silicon aluminum alloy, so that a uniform and continuous anodized film can be formed on its outer surface, thereby improving the protection effect and surface texture of the prepared product.
[0076] In the above technical solution, the preparation method of the container also includes demolding pretreatment. The demolding pretreatment specifically includes opening the mold, taking out the container matrix and cooling it after the molten metal in the cavity is formed into the container matrix, and processing the cooled container matrix to a preset size and / or preset accuracy. When the container matrix is processed by the die-casting liquid forging composite process, some processing allowances are generally reserved for the container matrix. Therefore, after the container is basically prepared and formed, the container matrix can be processed into the size and accuracy required by the drawing (such as roughness, flatness and coaxiality, etc.) by machining and other methods.
[0077] In the above technical solution, the preparation method of the container also includes roughness treatment. The roughness treatment specifically includes: after the container substrate is taken out from the mold, the inner and outer surfaces of the container substrate are subjected to roughness treatment until the roughness Ra of the inner and outer surfaces of the container substrate is greater than or equal to 2μm and less than or equal to 5μm. Furthermore, this step is generally performed after the demolding pretreatment. If there is no demolding pretreatment step, the roughness treatment can be performed directly after the part is demolded. By performing roughness treatment on the container substrate, the surface quality of the container substrate can be guaranteed, and preparations can be made for subsequent coating spraying on the container substrate.
[0078] Further, the roughening treatment includes sandblasting and / or grinding.
[0079] Furthermore, the preparation method of the container also includes forming a non-stick coating. The step of forming the non-stick coating specifically includes: forming a non-stick coating on the inner wall surface of the container substrate. The non-stick performance of the inner wall surface of the container can be improved by providing the non-stick coating. The non-stick coating can specifically include one or more of PTFE coating, PFA coating, PEEK coating, and ceramic coating. Furthermore, after the roughness treatment, the non-stick coating is formed on the inner wall surface of the container substrate, that is, the roughness treatment is performed first, and then the non-stick coating is formed.
[0080] Furthermore, the preparation method also includes degreasing the container substrate after the step of roughening and before the step of forming the non-stick coating. After the prepared container substrate is processed by machining or roughening, there will be some grease on the surface, so degreasing is required before forming the non-stick coating. The degreasing treatment can be high-temperature heating. At this time, the container can be heated. The specific heating temperature can be 350°C-420°C, and the heating temperature can last for 8min-15min. Of course, the degreasing treatment can also be carried out by other methods such as chemical degreasing.
[0081] In the above technical solution, the step of roughness treatment and the step of processing the cooled container base to a preset size and / or a preset precision are located before the step of anodizing the outer surface of the container base. That is, the steps of roughness treatment and demoulding pretreatment are performed first, and the anodizing treatment is performed last, because the anodizing treatment is to form a high-quality film layer on the surface, and this step is performed last, which can prevent the anodized film from being scratched or damaged due to the preparation of the non-stick coating, etc. after the preparation is completed.
[0082] In the above technical solution, the diameter of the holes in the container matrix is less than or equal to 1.5 mm, and the porosity of the preset holes in the container matrix is greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container matrix is formed, the number of holes in the unit area of 10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container matrix is greater than or equal to twice the diameter of each preset hole itself. This type of container matrix makes the bubbles relatively small, the interior of the parts is denser, and ensures the qualified rate of the product.
[0083] In a specific preparation method, the preparation process is as follows: after the molten metal in the cavity is formed into a container matrix, the mold is opened, the container matrix is taken out and cooled, and the cooled container matrix is processed to a preset size and / or preset accuracy; then degreasing treatment is performed, followed by sandblasting and other roughness treatments, and then a non-stick coating treatment is performed, and finally anodizing treatment is performed.
[0084] The following uses a cooking vessel as an example to further introduce the method for preparing a container provided by the present application and the container prepared by the method. Specifically:
[0085] The present invention belongs to the technical field of kitchen utensil production and manufacturing, and specifically relates to a cooking utensil production method that can better realize the functions of inner and outer coatings, reduce product defective rates, and simultaneously utilize an outer surface anodized layer to achieve high-grade texture and product recognition.
[0086] Among them, the vessel base is produced by a die-casting-liquid forging composite process, such as Figure 4 As shown, the production process includes the following steps:
[0087] S402, adding aluminum ingots according to the mass percentage of aluminum alloy components to melt, and then adopting a die-casting liquid forging composite process to form a corresponding cooking vessel, and then processing it to a specified size and accuracy according to the requirements of the drawing after it is removed from the mold and cooled.
[0088] S404, performing high-temperature degreasing on the cooking vessel and then performing non-stick coating treatment, wherein the heating temperature during high-temperature degreasing is 350°C-420°C and the heating time is 8min-15min;
[0089] S406, anodizing the outer surface of the cooking vessel to form a uniform, continuous and dense oxide film on the outer surface of the vessel.
[0090] Specifically, the die-casting-liquid forging composite process hydraulically injects molten aluminum into the mold cavity, dynamically adjusts the filling speed to reduce air entrapment, and then uses the extrusion rod in the mold to locally extrude and compensate for the shrinkage of the semi-solid casting formed in the cavity to increase its density.
[0091] When the corresponding cooking vessel is obtained by die casting-liquid forging composite process, the injection pressure of the molten metal is greater than or equal to 65MPa and less than or equal to 110MPa, the injection speed is greater than or equal to 5m / s and less than or equal to 8m / s, and the filling time of the molten metal is greater than or equal to 0.02s and less than or equal to 0.05s. When extruding at the preset position of the semi-formed part, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s.
[0092] Specifically, the Si content in the cast aluminum alloy is less than 0.5% in order to achieve an ideal anodizing effect.
[0093] Specifically, non-aluminum-silicon alloy is selected for aluminum casting in order to achieve an ideal anodizing effect. Since element Si cannot be completely removed during the melting and smelting process of aluminum ingots, the Si content must be controlled to be less than 0.5% in practice.
[0094] Specifically, the maximum diameter of a single hole inside a cooking pot produced by the die-casting-liquid forging composite process shall not exceed 1.5mm, and holes with a diameter less than 0.25mm shall not be counted. Within a unit area of 10cm×10cm, the number of holes shall not exceed 4, and the distance between two holes shall not be less than 5cm, and the distance between the center point of the hole and the surface of the casting shall not be less than 2 times the diameter of the hole itself.
[0095] Specifically, after the cooking utensils are removed from the mold and cooled, they are processed to the specified size and accuracy according to the requirements of the drawings, and then operated according to the following process flow: (1) the inside and outside of the utensils are sandblasted, and the surface roughness Ra after sandblasting is 2 microns to 5 microns; (2) high-temperature degreasing is performed, the heating temperature is 350°C to 420°C, and the heating time is 8min to 15min; (3) a non-stick coating is sprayed on the inside of the aluminum alloy, including but not limited to PTFE, PFA, PEEK, ceramic and other coatings that can achieve non-stick properties; (4) the outside is anodized to achieve rust prevention and high-grade texture.
[0096] This technology combines the two processes of die casting and liquid die forging, taking advantage of the respective advantages of low die casting cost and high liquid die forging casting quality, and creatively uses the die casting-liquid die forging composite process to manufacture cooking utensils, thereby improving the yield of the original die-casting aluminum alloy and enhancing the cost-effectiveness.
[0097] Die casting is a metal casting process that uses high pressure to force molten metal into a complex-shaped metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate.
[0098] Liquid die forging is a metal forming process that has both casting characteristics and is similar to die forging. It is a process that directly pours a certain amount of molten metal into the mold cavity and cools it under continuous mechanical static pressure. Liquid die forging technology can eliminate shrinkage cavities formed by cooling shrinkage and obtain high-strength parts with fine and uniform grains and dense structure, but the cost is relatively high. The punch extrusion pressure of liquid die forging is generally selected between 60MPa and 100MPa, the filling speed of the molten metal is controlled below 0.8m / s, the punch pressurization speed is between 0.1m / s and 0.4m / s, and the holding time is 10s to 30s.
[0099] The die-casting-liquid forging composite process injects the function of liquid forging by making targeted modifications to the die-casting technology. It reduces air entrapment by dynamically adjusting the filling speed during the die-casting process, and uses the extrusion rod in the mold to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal cools and shrinks. This greatly reduces product holes, and the risk of blistering or localized peeling of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience.
[0100] In addition, the die-casting-liquid forging composite process can use low-silicon aluminum alloy to die-cast complex structure products. The anodized layer on the surface of the low-silicon aluminum alloy is dense, uniform and continuous, which not only helps to improve the protection effect, but also can form a high-grade texture and unique product recognition.
[0101] Specifically, the following tests were performed on Example, Comparative Example 1 and Comparative Example 2.
[0102] Embodiment: A low silicon aluminum alloy 1050A is selected, and the content of each element (weight percentage) is Si: 0.17, Fe: 0.23, Zn: 0.05, Ti: 0.03, Al: balance. The cooking container is formed by a die casting-liquid forging composite process, and then CNC (Computer numerical control, numerical control machine tool) - sandblasting - degreasing - spraying non-stick coating inside the container - anodizing the outside of the container.
[0103] Comparative Example 1: A low silicon aluminum alloy 1050A was selected, and the content of each element (weight percentage) was Si: 0.17, Fe: 0.23, Zn: 0.05, Ti: 0.03, and Al: the remainder. The cooking container was formed by conventional die-casting process, and then CNC-sandblasting-degreasing-non-stick coating was sprayed inside the container-anodized outside the container.
[0104] Comparative Example 2: Aluminum-silicon alloy YL113 was selected, and the content of each element (weight percentage) was Si: 10.8, Fe: 0.8, Cu: 2.5, Zn: 1.6, and Al: balance. The cooking container was formed by conventional die-casting process, and then CNC-sandblasting-degreasing-non-stick coating was sprayed inside the container-anodized outside the container.
[0105] Test method: 50 cooking containers were produced in each of the above embodiments and comparative examples, and then the following tests were performed:
[0106] 1. Appearance inspection: Visually inspect the overall appearance and surface quality of the casting after demoulding. If the appearance quality is unqualified due to factors such as mold sticking and undercasting, it will be scrapped. The scrapped products will not be tested below.
[0107] 2. Coating blistering: Observe the visible blistering on the inner surface of the non-stick coating after it has cured, and calculate the proportion of blistering on the coating in the cooking vessel.
[0108] 3. Anodizing: including anodizing layer appearance test (visual inspection), film thickness measurement (film thickness meter), hardness test (Vickers hardness tester), where film thickness and hardness are the average values of multiple samples.
[0109] 4. Boiling vinegar test: Add 3% edible white vinegar into a container, boil it for 1 hour, then turn off the power and let it stand for 2 hours. This is one cycle. Repeat 7 cycles and check for coating shedding, discoloration, peeling and other adverse conditions.
[0110] Table 1: Test results of examples and comparative examples
[0111]
[0112] As shown in the test results in Table 1, OK means passing the test, and NG means failing the test. When comparative example 1 uses the traditional die-casting process to manufacture low-silicon aluminum, the scrap rate is very high due to the problems of mold sticking and poor fluidity. When the embodiment uses the composite process to manufacture the same low-silicon aluminum, such problems will not occur. When comparative example 2 uses aluminum-silicon alloy die-casting, all are qualified. In addition, the castings produced by the traditional die-casting process have relatively more internal defects and pores, resulting in a high blistering rate of the coating. After boiling vinegar, the risk of cracking and partial detachment of the coating increases, which can easily cause early failure. Since comparative example 2 uses non-aluminum-silicon alloy, the quality of the anodized film is poor, discontinuous, and not dense. The result fed back from the data is that the hardness is low and the average thickness of the film layer is thin.
[0113] In the description of this specification, the terms "connection", "installation", "fixation" and the like should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0114] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0115] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A container, characterized in that: include: A container base, wherein the container base is formed by a die-casting and liquid forging composite process; The anodic oxide film is located on the outer surface of the container substrate.
2. The container according to claim 1, characterized in that Also includes: The non-stick coating is located on the inner wall of the container base.
3. The container according to claim 1, characterized in that The weight percentage of Si in the container matrix is greater than or equal to 0 and less than or equal to 0.5%.
4. The container according to claim 1, characterized in that The container substrate comprises an aluminum-silicon alloy substrate; and / or The thickness of the anodized film is greater than or equal to 10 μm and less than or equal to 50 μm; and / or The wall thickness of the container base is greater than or equal to 2 mm and less than or equal to 12 mm.
5. The container according to any one of claims 1 to 4, characterized in that The diameter of the holes in the container matrix is less than or equal to 1.5 mm, the porosity of the preset holes in the container matrix is greater than 0 and less than or equal to 0.5%, the diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each of the preset holes and the outer surface of the container matrix is greater than or equal to twice the diameter of each of the preset holes.
6. A method for preparing a container, characterized in that: Used to prepare a container according to any one of claims 1 to 5, the preparation method comprising: Fill the molten metal into the mold cavity at a preset filling speed; When the molten metal in the mold cavity is formed into a semi-formed part, a preset portion of the semi-formed part is extruded until the molten metal in the mold cavity is formed into the container base; After the container base is taken out from the mold, the outer surface of the container base is anodized to form an anodized film that meets preset requirements on the outer surface of the container base.
7. The method for preparing a container according to claim 6, characterized in that: In the step of filling the molten metal into the mold cavity at a preset filling speed, the injection pressure is greater than or equal to 65 MPa and less than or equal to 110 MPa, the injection speed is greater than or equal to 5 m / s and less than or equal to 8 m / s, the filling time of the molten metal is greater than or equal to 0.02 s and less than or equal to 0.05 s, and the filling speed of the molten metal is greater than 0 and less than or equal to 0.8 m / s; and / or When extruding the preset part of the semi-formed part, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s.
8. The method for preparing a container according to claim 6, characterized in that: The molten metal includes a cast aluminum alloy molten metal, and the weight percentage of Si in the cast aluminum alloy molten metal is greater than 0 and less than or equal to 0.5%.
9. The method for preparing a container according to claim 6, characterized in that: Also includes: After the molten metal in the cavity is formed into the container base, the mold is opened, the container base is taken out and cooled, and the cooled container base is processed to a preset size and / or preset accuracy; and / or Roughness treatment: after taking out the container base from the mold, the inner and outer surfaces of the container base are subjected to roughness treatment until the roughness Ra of the inner and outer surfaces of the container base is greater than or equal to 2 μm and less than or equal to 5 μm. After the roughness treatment, a non-stick coating is formed on the inner wall surface of the container base.
10. The method for preparing a container according to claim 9, characterized in that: The preparation method further comprises, after the step of roughness treatment and before the step of forming the non-stick coating, performing a degreasing treatment on the container substrate; and / or The step of roughening the surface and the step of machining the cooled container substrate to a preset size and / or a preset accuracy are located before the step of anodizing the outer surface of the container substrate.
11. The method for preparing a container according to claim 10, characterized in that: The roughness treatment comprises sandblasting; and / or The degreasing treatment includes heating the container base, wherein the heating temperature is greater than or equal to 350° C. and less than or equal to 420° C., and the heating time is greater than or equal to 8 minutes and less than or equal to 15 minutes.
12. The method for preparing a container according to any one of claims 6 to 11, characterized in that: The diameter of the holes in the container matrix is less than or equal to 1.5 mm, the porosity of the preset holes in the container matrix is greater than 0 and less than or equal to 0.5%, the diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each of the preset holes and the outer surface of the container matrix is greater than or equal to twice the diameter of each of the preset holes.