Process method for cyclic utilization of ternary precursor washing liquid alkali for multiple times
Through the multiple recycling process of ternary precursor washing liquid alkali, the problems of water consumption and alkali consumption in the existing technology are solved, the washing efficiency and impurity removal effect are improved, the production and sewage treatment costs are reduced, and the positive electrode material is ensured. electrochemical properties.
Patent Information
- Application Number
- CN202410271071.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-12
AI Technical Summary
The existing ternary precursor washing process consumes a large amount of water and alkali, resulting in high production costs and sewage treatment costs, and it is difficult to effectively remove impurities and ions, affecting the electrochemical performance of the cathode material.
The process of multiple recycling of ternary precursor washing liquid alkali is adopted. Through the first-level washing, circulating alkali washing, water washing and diaphragm pressing, the recycling of alkali liquid is controlled, the consumption of liquid alkali and pure water is reduced, and the washing efficiency is improved. .
It significantly reduces the consumption of liquid alkali and pure water, reduces the cost of production and sewage treatment, improves the removal efficiency of impurity ions, and ensures the electrochemical performance of the cathode material.
Smart Images

Figure CN118925344A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ternary precursor material washing treatment, and in particular to a process method for multiple recycling of ternary precursor washing liquid alkali. Background Art
[0002] Precursor is one of the important raw materials for producing positive electrode materials for lithium-ion batteries. 80% of the performance indicators of the precursor will be directly transferred to the positive electrode material, and the impurity content will directly affect the electrochemical performance of the positive electrode material. At present, the industry's precursors are mainly based on wet synthesis. Nickel sulfate, cobalt sulfate, manganese sulfate, liquid alkali, and ammonia water are fed into the reactor in parallel. The ternary precursor is prepared by adjusting parameters such as the stirring frequency and the reactor temperature. After the synthesis, the ternary precursor is filtered and washed by a filter press. During the synthesis process, the sodium ions and sulfate ions in the raw materials will enter the ternary precursor with the complex precipitation reaction. If more impurity ions enter the positive electrode material with the ternary precursor, it will seriously affect the capacity and cycle life of the positive electrode material. Therefore, the precursor is washed after the synthesis to remove residual sodium ions and sulfate ions.
[0003] At present, the commonly used technology in the industry is to remove the mother liquor, alkali wash and water wash the ternary precursor slurry. Specifically, the mother liquor is removed by pressure filtration through the filter press washing equipment, and the filter cake is washed with a dilute alkali solution to remove sulfate, and then the sodium ions are removed by pure water washing. The above method can effectively remove residual sodium ions and sulfate ions, but the water consumption per ton of product is 10-20m³, and the alkali consumption is 100-200Kg. There are problems with high alkali and water consumption in the washing process.
[0004] Therefore, it is necessary to develop an efficient washing method that can significantly reduce the consumption of liquid alkali and pure water and improve washing efficiency while controlling the sodium ion and sulfate ion contents to maintain the current levels. Summary of the invention
[0005] The purpose of the present invention is to provide a highly efficient process for multiple recycling of ternary precursor washing liquid alkali.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a process for multiple recycling of ternary precursor washing liquid alkali, comprising the following steps: Step 1, preparation before primary washing: Turn on the 80-100℃ pure water pump and add 2.0±0.1m pure water into the alkali solution preparation tank. During the water adding process, open the alkali adding valve and add 700±100L liquid alkali through the flow meter to prepare an alkali solution with a concentration of 20-25g / L and a alkali solution temperature of 70-90℃; Step 2, primary washing feed: The precursor slurry obtained by the coprecipitation reaction is continuously transferred from the buffer tank to the washing equipment, and the mother liquid discharge valve of the washing equipment is kept open. After 5-10 minutes, the filter cake layer in the washing equipment is fully formed; Step 3, mother liquor removal: Keep the mother liquor discharge valve of the washing equipment open, stop feeding, perform solid-liquid separation, and keep the solid material in the filter plate cavity of the washing equipment; Step 4: Wash once: The mother liquor is discharged from the washing equipment through the mother liquor discharge pipe of the washing equipment and enters the mother liquor waste water tank. The washing equipment is washed once, and the washing water goes to the mother liquor waste water tank; Step 5: Circulating alkaline washing: Use the liquid alkali in the alkali solution preparation tank to circulate alkali washing on the filter cake in the washing equipment. The circulating alkali washing volume is 20m³. The liquid alkali after washing is returned to the alkali solution preparation tank for storage and washing of the next batch of materials. Step 6, secondary washing: The filter cake in the washing equipment is washed twice with water, and the secondary washing volume is 15m³; Step 7, diaphragm pressing: When the filter cake is compressed to the upper limit of squeezing, close the squeezing valve, and the squeezing valve closing limit indicator light is on. When the squeezing pressure drops to the lower limit of the pressure gauge, open the squeezing valve again. When the display setting is the same as the actual one, the diaphragm squeezing is completed. Step 8: Horn blowing: Blow air on the filter cake; Step nine, pull the plate to unload: The blown material is discharged into the slurry tank and enters the next process; When washing subsequent batches of materials, no new alkali is prepared, and steps 2 to 9 are repeated for each batch of materials; When the sulfate concentration in the alkali solution after alkali washing is greater than 0.4 g / L, the alkali solution is discharged and the recycling of the alkali solution is stopped.
[0007] The relevant contents in the above technical solution are explained as follows: 1. In step 1, the washing water volume is 5m³ per time.
[0008] 2. In step 5, the volume ratio of liquid alkali washing volume to precursor slurry is 0.6-0.8, and the alkali washing temperature is 60-90°C.
[0009] 3. Before washing each batch of materials, maintain the alkali concentration in the liquid alkali preparation tank at 20-25g / L by adding liquid alkali.
[0010] 4. After the alkali solution has been circulated and washed for 8 to 10 batches, the alkali solution is discharged and the circulation of the alkali solution is stopped.
[0011] The working principle of the present invention is: There is almost no way to remove impurities that form mixed crystals or solid solutions with the ternary precursor crystals, but impurities generated by side reactions can be removed by strictly controlling the crystallization conditions. Common methods include water washing and alkali washing. Impurities introduced by adsorption on the crystal surface are often removed by water washing, while impurities introduced by inclusion can be removed by alkali washing.
[0012] Water washing: The water washing of impurity ions can be composed of the following processes: ① The impurity ions overcome the adsorption effect of the crystal surface and migrate out from the crystal interface, and form a saturated layer at the interface between the impurity ions and water; ② Under the action of diffusion, the impurity ions diffuse from the saturated layer to the unsaturated layer, and then diffuse into the water to dissolve.
[0013] The adsorption of impurities on the crystal surface is an exothermic reaction. The lower the temperature, the easier it is for the impurity ions to be adsorbed and the more difficult it is for the impurity ions to migrate out. Therefore, the higher the water washing temperature, the better the impurity removal effect.
[0014] Ion diffusion refers to the diffusion of ions from high concentration to low concentration through their own concentration difference. The greater the concentration difference, the faster the diffusion rate. Therefore, for the same amount of crystals, the greater the water washing volume, the greater the concentration difference, the faster the rate of impurities migrating into the water, and the easier it is to remove the impurities. The higher the temperature, the greater the thermal motion rate of the ions and the faster the diffusion rate. Therefore, the higher the water temperature, the faster the rate of impurities migrating into the water and the easier it is to remove the impurities.
[0015] Alkali washing: Impurities hidden inside the crystal cannot be removed by direct water washing, but must be removed by alkali washing.
[0016] Alkaline cleaning requires OH - Re-entering the crystal will contain SO4 2- However, after the crystallization is completed, the OH in the mother liquor - After the reaction is basically complete, the crystals can be separated from the mother liquor and washed in a certain concentration of NaOH solution. The alkaline washing process can be divided into the following two steps: ① OH - Through ion exchange adsorption into the adsorption layer of the crystal surface interface phase, the SO4 2- ② OH in the adsorption layer - Diffusion into the crystal completes the transformation of the crystal form, while the SO4 2- Replaced to the adsorption layer on the crystal surface.
[0017] During the alkaline washing process, OH - The higher the concentration, the faster the solution diffusion rate, the easier it is to enter the adsorption layer on the crystal surface. The higher the alkaline washing temperature, the faster the ion diffusion rate and the better the washing effect. Alkaline washing with NaOH solution is also beneficial for washing SO42- impurity ions on the crystal surface, but it will also introduce OH on the crystal surface. -Therefore, the concentration of NaOH solution should not be too high. After the alkaline washing process is completed, it is combined with water washing to effectively reduce SO4 on the surface and inside of the crystal. 2- Impurity ions.
[0018] The alkali solution circulation washing process of the technical solution of the present invention is as follows: the alkali solution enters from the alkali solution preparation tank through the liquid inlet pipe of the washing equipment, is discharged from the liquid outlet of the washing equipment after fully filtering the filter cake, and the discharged alkali solution returns to the alkali solution preparation tank through valve control to form a cycle, and the alkali washing amount is controlled by time. The last alkali solution recycling washing method is direct discharge alkali washing, the alkali solution enters through the liquid inlet pipe of the washing equipment, is discharged from the liquid outlet after fully filtering the filter cake, and enters the waste alkali tank for external discharge after switching the valve.
[0019] Due to the application of the above technical solution, the present invention has the following advantages and effects compared with the prior art: 1. At present, the industry adopts a single direct discharge alkali washing method, that is, the configured liquid alkali is only washed once in the filter press washing process, and the liquid alkali after washing is treated as production wastewater, which has high production costs and sewage treatment costs. This patent realizes the configuration of liquid alkali for multiple batches of washing, reducing the production cost and sewage treatment cost of nickel-cobalt-manganese ternary precursors.
[0020] 2. This patent solves the problem of the enrichment of impurity sodium and sulfur elements during the preparation of multiple batches of liquid alkali for cyclic alkali washing, resulting in unqualified product indicators.
[0021] 3. The purpose of pH value control is to control the concentration of hydroxide ions in liquid alkali during the circulating alkali washing process. If the ion concentration is too low, the washing effect and sulfate ion removal effect will be poor. If the ion concentration is too high, sodium ions will easily be enriched, resulting in excessive sodium ion indicators. This technical solution explores and determines the optimal pH value control during the preparation of multiple batches of liquid alkali for cyclic use.
[0022] 4. After the material is washed by the technical solution of the present invention, it is measured that the sodium and sulfur content in the material is basically consistent before and after the comparison trend, and the material washing effect is good. The present invention automatically controls the flow direction of the alkali solution during the alkali washing process, realizes the recycling and discharge of the alkali solution, which not only reduces the cost of liquid alkali consumption, but also reduces the cost of sewage treatment. Because the temperature of the alkali solution will decrease during the storage process, the present invention can increase the number of recycling times in continuous batch washing and washing processes with low temperature requirements, which has great advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The process flow diagram of the present invention for the multiple recycling of the ternary precursor washing liquid alkali DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with the accompanying drawings and embodiments: The present invention will be further described below in conjunction with the accompanying drawings and embodiments: Embodiment: A process for recovering precursor materials from a ternary precursor mother liquor, the process is as follows Figure 1 As shown: Buffer tank: used to store qualified materials produced by the upstream process of the first-level washing process and filtered materials intercepted in the mother liquor of the first-level washing process.
[0025] Washing equipment: used for solid-liquid separation / washing of materials in the primary washing process.
[0026] Pure water tank: used to store pure water for washing process.
[0027] Liquid alkali preparation tank: used for the preparation of liquid alkali in the washing process and the storage of circulating alkali washing liquid.
[0028] Mother liquor wastewater tank: used for storing mother liquor and alkaline washing liquid in washing process.
[0029] Washing liquid wastewater tank: used for storing washing wastewater from the washing process.
[0030] Pulping tank: used for storage of washed qualified materials.
[0031] Preparation before feeding the first-level washing: turn on the 90℃ pure water pump and add 2.0±0.1m pure water into the alkali solution preparation tank. During the water adding process, open the alkali adding valve and add 700±100L liquid alkali through the flow meter. The alkali solution is prepared with a concentration of 20-25g / L. The temperature of the prepared alkali solution is controlled at 60-90℃. Samples are taken to test the alkali solution concentration (the sodium ion content of the initial prepared liquid alkali is in the range of 11-13gl / L, and the initial sulfate concentration is <0.5g / L).
[0032] First-stage washing feeding: open the transfer valve of buffer tank 1 and the feed valve of washing equipment 1, start the transfer pump of buffer tank 1, the pump frequency is 35Hz, and start feeding. After 5-10 minutes, the filter cake layer of washing equipment 1 is fully formed, and adjust the transfer pump frequency to 40-50Hz.
[0033] Mother liquor removal: During the feeding process, keep the mother liquor discharge valve of the washing equipment open, and the feeding is completed; open the "pressing" of the washing equipment to separate the solid and liquid, and the solid material remains in the filter plate cavity of the washing equipment.
[0034] One water wash: the mother liquor is discharged from the washing equipment through the mother liquor discharge pipe and enters the mother liquor wastewater tank. The washing equipment performs one water wash. The washing water volume is 5m³, and the washing water goes to the mother liquor wastewater tank.
[0035] Circulating alkali washing: Turn on the circulating alkali washing tank pump to carry out circulating alkali washing on the filter press filter cake. The circulating alkali washing volume is 20m³, the volume ratio of liquid alkali washing volume to precursor slurry is 0.6-0.8, the alkali washing temperature is 60-90℃, and the washing liquid alkali is returned to the filter press circulating alkali washing tank for storage to wash the next batch of materials.
[0036] Secondary water washing: Secondary water washing is to remove the residual alkali from the circulating alkali washing. Start the filter press pure water tank pump to start the secondary water washing. The secondary water washing volume is 15m³.
[0037] Diaphragm pressing: Click the diaphragm pressing start button, the diaphragm pressing valve is connected, the pressing valve open limit indicator light is on, and the filter press further compresses the filter cake. When the pressing pressure reaches the upper limit of the pressing, the pressing valve is closed, and the pressing valve close limit indicator light is on. When the pressing pressure drops to the lower limit of the pressure gauge, the pressing valve is opened again. When the display setting is the same as the actual cycle, it means that the diaphragm pressing is completed and the machine automatically ends the pressing state.
[0038] Corner blowing: Press the blowing button to blow air to the filter cake. When the specified time is reached, the operation ends.
[0039] Pull plate unloading: Press the pull plate unloading button, the pull plate indicator light will light up, the pull plate system will start working, the pull plate oil pump motor will start, the pull plate inlet solenoid valve will be energized, the pull plate mechanism will move forward, and when the set time is reached, the solenoid valve will be reversed, the pull plate retracting solenoid valve will be energized, and the pull plate mechanism will move backward. This cycle will continue until the last plate is pulled, the pull plate mechanism will trigger the pull plate return proximity switch, the pull plate will return, and it will retreat to the pull plate stop proximity switch. When the pull plate is finished, the pull plate motor will stop, and the material will be unloaded to the filter press pulping tank to enter the next process.
[0040] Washing of the 2nd to 8th batches of materials: the steps are omitted, no new alkali is prepared, and recycled liquid alkali is used for circulation washing. During the 4th batch of circulation washing, 100L of liquid alkali is added to the liquid alkali preparation tank.
[0041] The concentration range of sodium ion at the end of the second batch of cycle washing was (9-11 g / L) and the concentration range of sulfate ion was (0.5-0.9 g / L).
[0042] The sodium ion concentration range at the end of the third batch of cycle washing was (7-9 g / L) and the sulfate ion concentration range was (1.0-1.4 g / L).
[0043] The sodium ion concentration range at the end of the 4th batch of cycle washing was (5-7 g / L) and the sulfate ion concentration range was (1.5-1.9 g / L).
[0044] The sodium ion concentration range at the end of the fifth batch of cycle washing was (9-11 g / L) and the sulfate ion concentration range was (2.0-2.4 g / L).
[0045] The sodium ion concentration range at the end of the 6th batch of cycle washing was (7-9 g / L) and the sulfate ion concentration range was (2.5-2.9 g / L).
[0046] The sodium ion concentration range at the end of the 7th batch of cycle washing was (5-7 g / L) and the sulfate ion concentration range was (3.0-3.4 g / L).
[0047] The sodium ion concentration range at the end of the 8th batch of cycle washing was (3-5 g / L) and the sulfate ion concentration range was (3.5-3.9 g / L).
[0048] At the end of the 8th batch of circulating alkaline washing, turn on the alkali liquid pump, and the alkali liquid enters the washing equipment through the liquid inlet pipe of the filter press. The alkali washing liquid goes to the mother liquor wastewater tank, and the process of configuring liquid alkali for recycling 8 batches of materials is completed.
[0049] In specific implementation, before washing each batch of materials, the alkali concentration in the liquid alkali preparation tank can be maintained at 20-25 g / L by adding liquid alkali, or liquid alkali can be added only before washing the 4th to 6th batches of materials.
[0050] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for multiple recycling of ternary precursor washing liquid alkali, Features: The following steps are involved: Step 1, preparation before primary washing: Turn on the 80-100℃ pure water pump and add 2.0±0.1m pure water into the alkali solution preparation tank. During the water adding process, open the alkali adding valve and add 700±100L liquid alkali through the flow meter to prepare an alkali solution with a concentration of 20-25g / L and a alkali solution temperature of 70-90℃; Step 2, primary washing feed: The precursor slurry obtained by the coprecipitation reaction is continuously transferred from the buffer tank to the washing equipment, and the mother liquid discharge valve of the washing equipment is kept open. After 5-10 minutes, the filter cake layer in the washing equipment is fully formed; Step 3, mother liquor removal: Keep the mother liquor discharge valve of the washing equipment open, stop feeding, perform solid-liquid separation, and keep the solid material in the filter plate cavity of the washing equipment; Step 4: Wash once: The mother liquor is discharged from the washing equipment through the mother liquor discharge pipe of the washing equipment and enters the mother liquor waste water tank. The washing equipment is washed once, and the washing water goes to the mother liquor waste water tank; Step 5: Circulation alkaline washing: Use the liquid alkali in the alkali solution preparation tank to circulate alkali washing on the filter cake in the washing equipment. The circulating alkali washing volume is 20m³. The liquid alkali after washing is returned to the alkali solution preparation tank for storage and used for washing the next batch of materials. Step 6, secondary washing: The filter cake in the washing equipment is washed twice with water, and the secondary washing volume is 15m³; Step 7, diaphragm pressing: When the filter cake is compressed to the upper limit of squeezing, close the squeezing valve, and the squeezing valve closing limit indicator light is on. When the squeezing pressure drops to the lower limit of the pressure gauge, open the squeezing valve again. When the display setting is the same as the actual one, the diaphragm squeezing is completed. Step 8: Horn blowing: Blow air on the filter cake; Step nine, pull the plate to unload: The blown material is discharged into the slurry tank and enters the next process; When washing subsequent batches of materials, no new alkali is prepared, and steps 2 to 9 are repeated for each batch of materials; When the sulfate concentration in the alkali solution after alkali washing is greater than 0.4 g / L, the alkali solution is discharged and the recycling of the alkali solution is stopped.
2. The process for multiple recycling of ternary precursor washing liquid alkali according to claim 1, Features: In step 1, the washing water volume is 5m³ per time.
3. The process for multiple recycling of ternary precursor washing liquid alkali according to claim 1, Features: In step five, the volume ratio of the liquid alkali washing amount to the precursor slurry is 0.6-0.8, and the alkali washing temperature is 60-90°C.
4. The process for multiple recycling of ternary precursor washing liquid alkali according to claim 1, Features: Before washing each batch of materials, the alkali concentration in the alkali preparation tank is maintained at 20-25g / L by adding liquid alkali.
5. The process for multiple recycling of ternary precursor washing liquid alkali according to claim 1, Features: After the alkali solution has been circulated and washed for 8 to 10 batches, the alkali solution is discharged and the circulation of the alkali solution is stopped.
Citation Information
Patent Citations
Method for reducing sulfur content of nickel-cobalt-manganese ternary positive electrode material precursor
CN111807421A
Automatic washing control system for ternary lithium ion battery precursor and use method of automatic washing control system
CN115663290A