Preparation method and application of porous organic filter aid

By alkalizing, sulfonating and foaming the pulp fiberboard, porous organic filter aids were prepared, which solved the problems of existing filter aids being prone to cracking, expensive, and lignin soluble in oil, achieving high efficiency and environmental protection Filtering effects and resource recycling.

CN118925345APending Publication Date: 2024-11-12SUZHOU BEILIN MICROFIBER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411218180.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing filter aids such as celite filter aids are prone to cracking, granular paper fiber filter aids are expensive, wood powder filter aids are non-porous, and lignin is soluble in cooling oil, which cannot meet filtration technical indicators and environmental protection requirements.

Method used

Through the process steps of alkalizing, sulfonation, foaming and drying of the pulp fiberboard, porous organic filter aids are prepared to enhance the hydrophilicity and reactivity of the fibers, form a uniform foam structure, and improve filtration efficiency and permeability.

Benefits of technology

It realizes the preparation of porous filter aids with low cost and environmental protection, improves filtration efficiency and cleanliness, reduces environmental pollution and production costs, adapts to industrial filtration needs, and has good resource recycling and reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925345A_ABST
    Figure CN118925345A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a porous organic filter aid, and relates to the technical field of filter aid preparation, and the preparation method comprises the following steps: S01, alkalization of a paper pulp fiberboard, S02, sulfonation of wet expanded loose alkalized fibers, S03, foaming of sulfonated viscose, S04, drying of a foaming body, S05, crushing of the dried foaming body, and S06, sorting of the crushed foaming body. The filter aid with a porous structure is prepared through a series of process steps of alkalization, sulfonation, foaming, drying and the like by using a paper pulp fiberboard with relatively low cost as a raw material, and the structure not only improves the filtering efficiency and permeability, but also enhances the hydrophilicity and reactivity of fibers, so that the filter aid has a good application prospect. Compared with the traditional diatomite, granular paper fiber and wood powder filter aid, the filter aid has the advantages that the influence on the environment is reduced in the preparation process, and meanwhile, different industrial filtering requirements can be met by optimizing process parameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filter aid preparation, in particular to a preparation method and application of a porous organic filter aid. Background Art

[0002] Filter aid is a filter agent, a consumable product for filtering and separating solid-liquid mixtures. It is mainly used as a filter aid for filtering rolling mill cooling oil in mechanical processing.

[0003] The filter aids currently available on the market include diatomaceous earth filter aids with porous structures, granular fiber organic filter aids prepared from needle-like paper fibers, and selected wood powder filter aids. Diatomaceous earth filter aids are inorganic materials with high rigidity and poor flexibility. They are easy to compact when used for filtering, and the filter cake is easy to crack. The solid-liquid mixture will leak through the cracks, which does not meet the requirements of filtering technical indicators. At the same time, because it is an inorganic material, the treatment of solid waste after filtration is also an environmental issue. Granular paper fiber filter aids are a mixture of a large amount of granular fibers and a small amount of needle-like fibers. They have good toughness and the filter cake does not crack. They are the most ideal filter aids, and the solid waste treatment also meets environmental protection requirements, but they are expensive. Selected wood powder filter aids are organic materials with less rigidity than diatomaceous earth, but they are not porous. Wood powder fibers are relatively fluffy. When filtering, fine particles are easy to leak through the gaps in the fluffy wood powder, which does not meet the requirements of filtering technical indicators. At the same time, the lignin in the wood powder will also be slightly dissolved in the cooling oil, polluting the cooling oil

[0004] In summary, it is necessary to develop a new filter aid that overcomes the shortcomings of diatomaceous earth filter cakes that are easy to crack, granular paper fiber filter aids that are expensive, wood powder filter aids that are non-porous, and lignin that is slightly soluble in cooling oil. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of a porous organic filter aid, which solves the problems in the background technology that diatomaceous earth filter cake is easy to crack, granular paper fiber filter aid is expensive, wood powder filter aid is non-porous and lignin is slightly soluble in cooling oil.

[0006] To achieve the above objectives, the present invention is implemented by the following technical scheme: a preparation method and application of a porous organic filter aid, the steps of which are as follows:

[0007] S01. Alkalization of pulp fiberboard: The pulp fiberboard is thoroughly cleaned and pretreated to remove impurities and non-fiber components, and the pretreated fiberboard is reacted with an alkalizer, which uses sodium hydroxide (NaOH) or sodium sulfate (Na2SO4) to deeply dissociate and swell the fibers;

[0008] S02. Sulfonation of wet expanded loose alkalized fibers: The alkalized fibers are fully washed and neutralized to remove the residual alkalizer, and the alkalized wet loose fibers are subjected to a sulfonation chemical reaction to enhance the hydrophilicity and reactivity of the fibers by introducing sulfonic acid groups to generate sulfonated viscose;

[0009] S03 sulfonated viscose foaming: the sulfonated viscose is added to the foaming agent for foaming, and the foaming agent is decomposed and released by physical heating or mechanical stirring to form a uniform foam structure to obtain a foam, wherein the foaming agent is NH4HCO3 powder;

[0010] S04 foam drying: the foamed viscous body is dried to remove moisture therein to form a dry foam;

[0011] S05. The dried foam is crushed: The dried foam is crushed by a crusher to reduce its particle size for subsequent sorting and application;

[0012] S06. Sorting of crushed foam: The obtained filter aid is evaluated for its performance, including its filtration efficiency, porosity, and mechanical strength indicators. The qualified filter aid is used in industrial filtration processes.

[0013] Preferably, the pulp fiberboard in S01 is a clean pulp fiberboard from which lignin has been removed and bleached; when the alkalizing agent is sodium hydroxide (NaOH), its proportion is 20%.

[0014] Preferably, the alkalization reaction experimental process is:

[0015] Take 50g of pulp fiberboard, put it into a two-necked reaction bottle, add 1000ml of 20% sodium hydroxide aqueous solution, and heat it in a water bath at a temperature of 40-50°C, so that the alkalization reaction can proceed fully and avoid cellulose degradation caused by high temperature. During the heating process, use a glass rod or a magnetic stirrer to continuously stir the mixture to ensure that the sodium hydroxide solution is in full contact with the pulp fiberboard and promote the uniformity of the reaction. The stirring speed should be moderate to ensure that the fiberboard and the solution are mixed evenly and to prevent fiber damage due to excessive shear force. The reaction is terminated after 1.0-1.5h, and the mixture is taken out to form a mixture of loose expanded fibers and solution. Pour out the solution (the solution can be recycled) to obtain wet expanded loose fibers.

[0016] Preferably, in the S02, the sulfonating agent for the wet expanded loose fiber sulfonation reaction is carbon disulfide (CS2), and the sulfonation reaction experimental process is:

[0017] First, put the wet expanded loose fibers into a two-necked reaction bottle, then add 360 ml of tap water, stir evenly, then add 8-10 ml of carbon disulfide (CS2), and continue stirring for 30-45 minutes. When the expanded loose fibers are completely dissolved into a viscous paste, sulfonated viscose is obtained. During the sulfonation reaction, the system will produce violent exothermic phenomenon. The water bath temperature needs to be controlled at 80-95°C to compensate for the heat loss and maintain the temperature required for the reaction.

[0018] Preferably, in the S03, when the wet expanded loose fibers are completely dissolved into a viscous paste, 4 g of ammonium bicarbonate (NH4HCO3) powder, a foaming agent, is added. The gas generated by the decomposition of ammonium bicarbonate (NH4HCO3) will promote the fiber material to form a porous structure. Subsequently, the mixture is continued to be uniformly stirred to ensure that the sulfonated viscose and the foaming agent are fully mixed to form a uniform foaming precursor solution. The foaming precursor solution is discharged into a preheated foaming tank. The temperature of the foaming tank is controlled at 80-95°C for 1.5-3.0 hours to obtain a foam.

[0019] Preferably, in S04, the foam is dried, and the drying process can be carried out by hot air drying, vacuum drying, natural drying or freeze drying. In the drying process, natural drying is further preferred. The drying rate and temperature need to be controlled, wherein the temperature is 9.0°C, the air flow velocity is 1.0 m / s, and the humidity is 64% to ensure the integrity and stability of the foam structure. The water content is less than 15% to be qualified.

[0020] Preferably, in S05, the dried foam is crushed by a crusher at a temperature of 5 to 40°C and a humidity of 10% to 80%. The crusher is a general crusher with a rotation speed of 960 r / min to 3400 r / min and a power of 4 kW to 15 kW.

[0021] Preferably, in S06, the crushed foam is sorted, and the sorting machine is a screen sorter or a grading machine sorter for sorting. Further, a screen sorter is preferred, and the screen sorter uses a two-layer screen to separate materials of different particle sizes through the relative movement of the material on the screen and the difference in the size of the screen holes.

[0022] Preferably, the aperture of the upper sieve is 0.18 mm, and the aperture of the lower sieve is 0.05 mm. After sorting, more than 85% of the volume particle size is distributed in the range of 0.05 mm to 0.18 mm, the bulk density is 140 to 280 g / L, and the permeability is 3.0 to 8.0D. This particle size filter aid can meet the filtration requirements.

[0023] Preferably, the method of using the rolling mill cooling oil in mechanical processing is as follows: a layer of clean porous organic filter aid is evenly laid on the filter cloth of the filtering equipment to prepare an ideal medium for filtration, and the rolling mill cooling oil containing impurities is slowly and evenly injected onto the filter aid to ensure that the oil product is in full contact with the filter aid. With the help of the porous structure of the filter aid, the solid impurities in the oil product are effectively retained, and the clean oil penetrates the filter cloth. After the oil product is completely penetrated, the solid waste on the filter cloth is removed to maintain the cleanliness of the filter medium and the filtration efficiency. The filtered clean oil product is collected and prepared to be put into use again, thereby reducing production costs and reducing environmental pollution.

[0024] The present invention provides a preparation method and application of a porous organic filter aid, which has the following beneficial effects:

[0025] The preparation method and application of a porous organic filter aid uses low-cost pulp fiberboard as a raw material and undergoes a series of process steps such as alkalization, sulfonation, foaming and drying to prepare a filter aid with a porous structure. This structure not only improves the filtration efficiency and permeability, but also enhances the hydrophilicity and reactivity of the fiber. Compared with traditional diatomaceous earth, granular paper fiber and wood powder filter aids, the filter aid reduces the impact on the environment during the preparation process. By optimizing the process parameters, it can adapt to different industrial filtration needs. In addition, it also has good resource recovery and reuse, reduces waste generation in the production process, helps to reduce production costs, reduces environmental pollution, and improves the cleanliness of oil products, thereby showing its unique advantages in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the process of the present invention;

[0027] Figure 2 This is a schematic diagram of a particle size analysis report of Example 1 of the present invention;

[0028] Figure 3 This is a schematic diagram of the particle size analysis report of Example 2 of the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the following examples, the raw materials used are bleached pulp fiberboard, tap water, sodium hydroxide (NaOH), carbon disulfide (CS2), ammonium bicarbonate (NH4HCO3)

[0031] Example 1

[0032] like Figure 1 , Figure 2 As shown, a method for preparing a clean porous organic filter aid comprises the following steps:

[0033] Step 1: Alkalization reaction of pulp fiberboard: Use a 2000ml two-necked reaction bottle, heat it in a water bath, take 50g of pulp fiberboard, cut the cardboard into small pieces that can be put into the bottle mouth, put them into the two-necked reaction bottle, add 1000ml of 20% sodium hydroxide aqueous solution, heat it in a water bath, stir while heating, keep the temperature at 47±3℃, and react for 1.0h before termination. At this time, the cardboard becomes a mixture of loose expanded fibers and sodium hydroxide solution. Take it out, separate the sodium hydroxide solution and discharge it into a measuring cup (the solution can be recycled) to obtain wet expanded loose alkalized fibers.

[0034] Step 2: Sulfonation of wet expanded loose alkalized fiber: first put the wet expanded loose alkalized fiber into a two-necked reaction bottle, then add 360ml of tap water, stir evenly, then add 8ml of CS2, continue stirring for 45 minutes, and when the expanded loose fiber is completely dissolved into a sticky paste, the sulfonated viscose is obtained. The sulfonation reaction is a violent exothermic reaction, and the water bath temperature is controlled at 92±3℃.

[0035] Step 3: When the wet expanded loose fibers are completely dissolved into a viscous paste, add 4g of foaming agent NH4HCO3 powder and continue stirring. When the sulfonated viscose and the foaming agent are evenly mixed, quickly discharge them into the foaming tank for foaming. The temperature of the foaming tank is controlled at 83±3℃ for 2.5 hours to obtain a foamed body.

[0036] Step 4: Dry the foam: Place the foam outdoors for natural drying. The foam is qualified if the moisture content is less than 15%.

[0037] Step 5: Crush the dried foam: Crush the foam using a general-purpose crusher.

[0038] Step 6: sorting the crushed foam body, the sorting machine uses a 2-layer screen sorting machine, the aperture of the upper screen is 0.18mm, the aperture of the lower screen is 0.05mm, and the volume particle size of more than 85% of the sorting is 0.05mm~0.18mm, the bulk density is 206.30g / L, and the permeability is 7.66D. The filter aid of this particle size can meet the filtration requirements.

[0039] Table 1 Sample bulk density after sorting in Example 1

[0040]

[0041] Table 2 Permeability of samples after sorting in Example 1

[0042]

[0043] Example 2

[0044] like Figure 1 , Figure 3 As shown, a method for preparing a clean porous organic filter aid comprises the following steps:

[0045] Step 1: Alkalization reaction of pulp fiberboard: use a 2000ml two-necked reaction bottle, heat it in a water bath, take 50g of pulp fiberboard, cut the cardboard into small pieces that can be put into the bottle mouth, put them into the two-necked reaction bottle, add 1000ml of 20% sodium hydroxide aqueous solution, heat it in a water bath, stir while heating, keep the temperature at 43±3℃, and react for 1.5h before termination. At this time, the cardboard becomes a mixture of loose expanded fibers and sodium hydroxide solution. Take it out, separate the sodium hydroxide solution and discharge it into a measuring cup (the solution can be recycled) to obtain wet expanded loose alkalized fibers.

[0046] Step 2: Sulfonation of wet expanded loose alkalized fiber: first put the wet expanded loose alkalized fiber into a two-necked reaction bottle, then add 360ml of tap water, stir evenly, then add 12ml of CS2, continue stirring for 30min, and when the expanded loose fiber is completely dissolved into a sticky paste, the sulfonated viscose is obtained. The sulfonation reaction is a violent exothermic reaction, and the water bath temperature is controlled at 83±3℃.

[0047] Step 3: When the wet expanded loose fibers are completely dissolved into a viscous paste, add 4g of foaming agent NH4HCO3 powder and continue stirring. When the sulfonated viscose and the foaming agent are evenly mixed, quickly discharge them into the foaming tank for foaming. The temperature of the foaming tank is controlled at 90±5℃ for 2.5 hours to obtain a foamed body.

[0048] Step 4: Dry the foam: Place the foam outdoors for natural drying. The foam is qualified if the moisture content is less than 15%.

[0049] Step 5: Crush the dried foam: Crush the foam using a general-purpose crusher.

[0050] Step 6: sorting the crushed foam body, using a classifier for sorting, adjusting the air volume of the sorting machine, and obtaining a filter aid with a volume particle size of more than 85% distributed between 0.05 mm and 0.18 mm, a bulk density of 201.14 g / L, and a permeability of 7.92D. This particle size filter aid can meet the filtration requirements.

[0051] Table 3 Bulk density of samples after sorting in Example 2

[0052]

[0053] Table 4 Permeability of samples after sorting in Example 2

[0054]

[0055] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0056] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a porous organic filter aid, characterized in that: The steps are as follows: S01. Alkalization of pulp fiberboard: The pulp fiberboard is thoroughly cleaned and pretreated to remove impurities and non-fiber components, and the pretreated fiberboard is reacted with an alkalizer, which uses sodium hydroxide (NaOH) or sodium sulfate (Na2SO4) to deeply dissociate and swell the fibers; S02. Sulfonation of wet expanded loose alkalized fibers: The alkalized fibers are fully washed and neutralized to remove the residual alkalizer, and the alkalized wet loose fibers are subjected to a sulfonation chemical reaction to enhance the hydrophilicity and reactivity of the fibers by introducing sulfonic acid groups to generate sulfonated viscose; S03 sulfonated viscose foaming: the sulfonated viscose is added to the foaming agent for foaming, and the foaming agent is decomposed and released by physical heating or mechanical stirring to form a uniform foam structure to obtain a foam, wherein the foaming agent is NH4HCO3 powder; S04 foam drying: the foamed viscous body is dried to remove moisture therein to form a dry foam; S05. The dried foam is crushed: The dried foam is crushed by a crusher to reduce its particle size for subsequent sorting and application; S06. Sorting of crushed foam: The obtained filter aid is evaluated for its performance, including its filtration efficiency, porosity, and mechanical strength indicators. The qualified filter aid is used in industrial filtration processes.

2. The method for preparing a porous organic filter aid according to claim 1, characterized in that: The pulp fiberboard in S01 is a clean pulp fiberboard that has been bleached after removing lignin; when the alkalizing agent is sodium hydroxide (NaOH), its component ratio is 20%.

3. The method for preparing a porous organic filter aid according to claim 1, characterized in that: The alkalization reaction experimental process is: Take 50g of pulp fiberboard, put it into a two-necked reaction bottle, add 1000ml of 20% sodium hydroxide aqueous solution, and heat it in a water bath at a temperature of 40-50°C, so that the alkalization reaction can proceed fully and avoid cellulose degradation caused by high temperature. During the heating process, use a glass rod or a magnetic stirrer to continuously stir the mixture to ensure that the sodium hydroxide solution is in full contact with the pulp fiberboard and promote the uniformity of the reaction. The stirring speed should be moderate to ensure that the fiberboard and the solution are mixed evenly and to prevent fiber damage due to excessive shear force. The reaction is terminated after 1.0-1.5h, and the mixture is taken out to form a mixture of loose expanded fibers and solution. Pour out the solution (the solution can be recycled) to obtain wet expanded loose fibers.

4. The method for preparing a porous organic filter aid according to claim 1, characterized in that: In the S02, the sulfonating agent for the wet expanded loose fiber sulfonation reaction is carbon disulfide (CS2), and the sulfonation reaction experimental process is: First, put the wet expanded loose fibers into a two-necked reaction bottle, then add 360 ml of tap water, stir evenly, then add 8-10 ml of carbon disulfide (CS2), and continue stirring for 30-45 minutes. When the expanded loose fibers are completely dissolved into a viscous paste, sulfonated viscose is obtained. During the sulfonation reaction, the system will produce violent exothermic phenomenon. The water bath temperature needs to be controlled at 80-95°C to compensate for the heat loss and maintain the temperature required for the reaction.

5. The method for preparing a porous organic filter aid according to claim 1, characterized in that: In the S03, when the wet expanded loose fibers are completely dissolved into a viscous paste, 4 g of ammonium bicarbonate (NH4HCO3) powder, a foaming agent, is added. The gas generated by the decomposition of ammonium bicarbonate (NH4HCO3) will promote the fiber material to form a porous structure. Subsequently, the mixture is continued to be uniformly stirred to ensure that the sulfonated viscose and the foaming agent are fully mixed to form a uniform foaming precursor solution. The foaming precursor solution is discharged into a preheated foaming tank. The temperature of the foaming tank is controlled at 80-95°C for 1.5-3.0 hours to obtain a foamed body.

6. The method for preparing a porous organic filter aid according to claim 1, characterized in that: In S04, the foam is dried. The drying process may be hot air drying, vacuum drying, natural drying or freeze drying. Natural drying is further preferred. The drying rate and temperature need to be controlled. The temperature is 9.0°C, the air flow velocity is 1.0 m / s, and the humidity is 64% to ensure the integrity and stability of the foam structure. The moisture content is less than 15% to be qualified.

7. The method for preparing a porous organic filter aid according to claim 1, characterized in that: In the step S05, the dried foam is crushed by a crusher at a temperature of 5 to 40°C and a humidity of 10% to 80%. The crusher is a general crusher with a rotation speed of 960 r / min to 3400 r / min and a power of 4 kW to 15 kW.

8. The method for preparing a porous organic filter aid according to claim 1, characterized in that: In the S06, the crushed foam is sorted, and the sorting machine is a screen sorter or a grading machine sorter. Further, the screen sorter is preferred. The screen sorter uses a two-layer screen to separate materials of different particle sizes through the relative movement of the materials on the screen and the difference in the size of the screen holes.

9. The method for preparing a porous organic filter aid according to claim 8, characterized in that: The aperture of the upper sieve is 0.18mm, and the aperture of the lower sieve is 0.05mm. After sorting, the filter aid has a volume particle size of more than 85% distributed between 0.05mm and 0.18mm, a bulk density of 140 to 280g / L, and a permeability of 3.0 to 8.0D. This particle size filter aid can meet the filtration requirements.

10. The use of a porous organic filter aid according to any one of claims 1 to 9, which is used for filtering rolling mill cooling oil in mechanical processing, and the method of use is: evenly laying a layer of clean porous organic filter aid on the filter cloth of the filtering equipment to prepare an ideal medium for filtration, slowly and evenly injecting the rolling mill cooling oil containing impurities onto the filter aid to ensure that the oil product is in full contact with the filter aid, with the help of the porous structure of the filter aid, the solid impurities in the oil product are effectively retained, and the clean oil penetrates the filter cloth, after the oil product is completely penetrated, the solid waste on the filter cloth is removed to maintain the cleanliness and filtration efficiency of the filter medium, and the filtered clean oil product is collected and prepared to be put into use again, thereby reducing production costs and reducing environmental pollution.