VOCs adsorbent and preparation method thereof

Through the multi-step treatment of waste molecular sieve, the problem of insufficient performance of existing adsorbents is solved, the effect of efficient VOCs removal is achieved, and the preparation cost is reduced.

CN118925697AActive Publication Date: 2024-11-12CHINA ENERGY GRP NINGXIA COAL IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410976178.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing VOCs adsorbents have poor adsorption performance and low adsorption capacity, making it difficult to effectively remove volatile organic compounds in the air.

Method used

By dissolving waste molecular sieve with aluminum and silicon dissolved treatment, a 13X molecular sieve is formed, and impregnated in silanizing reagent and nickel solution is carried out to form a nickel-modified 13X molecular sieve, and then hydrothermal reaction and calcination are carried out with titanium silicon molecular sieve to form a The core-shell structure is finally prepared by ion exchange and silanization modification treatment to prepare VOCs adsorbents with high adsorption properties.

Benefits of technology

It significantly improves the adsorption capacity and selectivity of VOCs adsorbents, enhances mechanical strength and thermal stability, reduces preparation costs, and is suitable for industrial emissions and indoor air purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954577980000131
    Figure BDA0004954577980000131
Patent Text Reader

Abstract

The invention provides a VOCs adsorbent and a preparation method thereof. The preparation method comprises the following steps: sequentially carrying out aluminum dissolving treatment and silicon dissolving treatment on a waste molecular sieve to obtain aluminum-rich liquid and silicon-rich liquid; the aluminum-rich liquid, the silicon-rich liquid and the seed crystal are sequentially subjected to gelation, aging and first hydrothermal crystallization, and the 13X molecular sieve is obtained; the method comprises the following steps: sequentially dipping a 13X molecular sieve in a silanization reagent solution and a nickel-containing solution to obtain a nickel-modified 13X molecular sieve; sequentially carrying out first hydrothermal reaction and roasting on the nickel modified 13X molecular sieve and the titanium silicalite molecular sieve precursor solution to obtain a core-shell structure 13X molecular sieve; carrying out ion exchange reaction on a cerium ion solution and the core-shell structure 13X molecular sieve, and then sequentially carrying out drying, alkaline solution treatment and first calcination to obtain a calcined 13X molecular sieve; and sequentially carrying out silanization modification and secondary calcination on the calcined 13X molecular sieve to obtain the VOCs adsorbent. The adsorbent prepared by the method has relatively high VOCs adsorption efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of VOCs adsorbent preparation, and in particular to a VOCs adsorbent and a preparation method thereof. Background Art

[0002] Molecular sieve is a kind of aluminosilicate, which has the characteristics of uniform pore size, regular crystal structure, rich pore system, large specific surface area, and good thermal stability. Molecular sieve is considered to be the preferred adsorbent material for removing oxygenated compounds from olefins. Among them, the pore size of FAU type (X, Y type) molecular sieve is about 0.74nm, especially X type molecular sieve can better remove oxygenated compound impurities from olefins. Therefore, there are many studies on X type molecular sieve, and X type molecular sieve has also been widely used in industrial practice.

[0003] First, the uniform and ordered microporous structure of the 13X molecular sieve enables it to accurately screen molecules, where the size and shape of the micropores can highly specifically adsorb molecules of a specific size and shape while excluding other molecules, which is very valuable in the separation and purification process in the chemical industry. For example, in the field of gas separation, the 13X molecular sieve can effectively separate target gases such as oxygen, nitrogen or carbon dioxide from a mixed gas flow. Secondly, the large specific surface area provides more active adsorption sites, increasing the adsorption capacity of the 13X molecular sieve. This means that within the same physical volume, the 13X molecular sieve can adsorb more substances, thereby improving the processing rate and efficiency. This feature is particularly important in the fields of liquid or gas purification, catalyst carriers, and storage media.

[0004] Therefore, 13X molecular sieves with uniform and orderly micropores, large specific surface area, large pore capacity and other characteristics not only show great potential in the traditional fields of chemical industry, oil and gas processing, but also show broad application prospects in emerging fields such as environmental protection, clean energy, life sciences, etc. For example, in industrial waste gas treatment, 13X molecular sieves can effectively remove harmful gases and volatile organic compounds (VOCs), and in the production of pharmaceuticals and refined chemicals, they can be used to improve the purity and yield of products.

[0005] With the intensification of industrialization, the emission of VOCs in the air continues to increase, posing a serious threat to human health and the environment. Common VOCs removal technologies include adsorption, catalytic combustion, etc. Among them, the adsorption method is widely used due to its simple operation and low cost. 13X molecular sieve has become the preferred adsorbent for VOCs removal due to its good thermal stability and large pore size. However, the traditional 13X molecular sieve still has room for improvement in the adsorption efficiency of VOCs. Summary of the invention

[0006] The main purpose of the present invention is to provide a VOCs adsorbent and a preparation method thereof, so as to solve the problems of poor adsorption performance and low adsorption capacity of VOCs adsorbents in the prior art.

[0007] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a VOCs adsorbent is provided, the preparation method comprising the following steps: step S1, subjecting the waste molecular sieve to aluminum dissolution treatment and silicon dissolution treatment in sequence to obtain aluminum-rich liquid and silicon-rich liquid; step S2, subjecting the raw materials including the aluminum-rich liquid, the silicon-rich liquid and the seed crystal to gelation treatment, aging treatment and first hydrothermal crystallization treatment in sequence to obtain a 13X molecular sieve; step S3, subjecting the 13X molecular sieve to a first impregnation treatment and a second impregnation treatment in a silanization agent solution and a nickel-containing solution in sequence, A nickel-modified 13X molecular sieve is obtained; step S4, a mixture including the nickel-modified 13X molecular sieve and the titanium silicon molecular sieve precursor solution is subjected to a first hydrothermal reaction and a roasting treatment in sequence to obtain a core-shell structure 13X molecular sieve; step S5, after an ion exchange reaction between the cerium ion solution and the core-shell structure 13X molecular sieve, the cerium ion solution is subjected to drying, an alkaline solution treatment, and a first calcination treatment in sequence to obtain a calcined 13X molecular sieve; and step S6, the calcined 13X molecular sieve is subjected to a silanization modification treatment and a second calcination treatment in sequence to obtain a VOCs adsorbent.

[0008] Further, in the above step S3: the time of the first impregnation treatment is 8 to 24 hours; and / or the time of the second impregnation treatment is 24 to 48 hours; preferably, the molar concentration of the silanization agent solution is 0.05 to 0.2 mol / L; and / or the molar concentration of the nickel-containing solution is 0.05 to 0.2 mol / L; preferably, the mass ratio of the 13X molecular sieve to the volume ratio of the silanization agent solution is 400 to 600:1 g / L; preferably, the mass ratio of the 13X molecular sieve to the volume ratio of the nickel-containing solution is 400 to 60 0:1g / L; preferably, the nickel-containing solution is a nickel nitrate solution and / or a nickel sulfate solution; preferably, the silanization agent is selected from any one or more of 3-aminopropyltriethoxysilane, tetraethoxysilane and tetramethoxysilane; preferably, step S3 also includes: subjecting the 13X molecular sieve obtained by the second impregnation treatment to a third calcination to obtain a nickel-modified 13X molecular sieve coated with a nickel nanoparticle layer; preferably, the atmosphere of the third calcination is hydrogen, the temperature of the third calcination is 500-600°C, and the time of the third calcination is 2-4h.

[0009] Further, in the above step S4, the temperature of the first hydrothermal reaction is 150-200°C, and the time of the first hydrothermal reaction is 12-24h; preferably, the temperature of the calcination treatment is 450-550°C, and the time of the calcination treatment is 4-8h; the titanium silicon molecular sieve precursor solution includes a first silicon source, a titanium source, a template, a fluorine complex and water, wherein the first silicon source, the titanium source, the template, the fluorine complex and the water are in a molar ratio of 1:0.04-0.1:0.1-0.3:0.03-0.06:20-50 Mixing; preferably, the mass ratio of the nickel-modified 13X molecular sieve to the volume ratio of the titanium silicon molecular sieve precursor solution is 400-600:1 g / L; preferably, the first silicon source is selected from any one or more of SiO2, Na2SiO3 and Si(OC2H5)4; preferably, the titanium source is selected from any one or more of TiO2, TiCl4 and Na2TiO3; preferably, the fluorine complex is selected from any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate and ammonium fluoride; preferably, the template is an organic amine and / or a quaternary ammonium salt.

[0010] Further, in the above step S5, the molar concentration of the cerium ion solution is 0.05-0.5 mol / L, calculated as cerium ions in the cerium ion solution, and the volume ratio of the mass of the core-shell structure 13X molecular sieve to the cerium ion solution is preferably 1-20:100 g / mL, and the cerium ion solution is preferably selected from any one or more of cerium chloride, cerium nitrate, cerium citrate, and cerium acetate; and / or the temperature of the ion exchange reaction is 45-60°C, and / or the time of the ion exchange reaction is 16-24h; the process of the alkaline solution treatment preferably includes: performing a third impregnation treatment on the dried molecular sieve in an alkaline solution, preferably the time of the third impregnation treatment is 1-3h, and the alkaline solution is preferably NaOH and / or KOH; preferably performing a first calcination treatment in an air atmosphere, preferably the temperature of the first calcination treatment is 400-600°C, and preferably the time of the first calcination treatment is 5-8h.

[0011] Furthermore, in the above step S6, the time of the silanization modification treatment is 8 to 24 hours; the volume ratio of the silane reagent and the solvent is preferably 1:5 to 10; the reagents used for the silanization modification treatment preferably include a silane reagent and a solvent; the silane reagent is preferably selected from any one or more of methyltrimethoxysilane, ethyltriethoxysilane and propenyltrimethoxysilane; the solvent is preferably selected from any one or more of ethanol, propanol and butanol; and / or the temperature of the second calcination treatment is 500 to 700°C, and the time of the second calcination treatment is 2 to 4 hours.

[0012] Furthermore, in the above step S2, the 13X molecular sieve contains silicon and aluminum, and the molar ratio of silicon to aluminum is 2.2 to 2.9:1; and / or the pore volume of the 13X molecular sieve is 0.3 to 0.5 cm 3 / g, and / or the specific surface area of ​​13X molecular sieve is 700-950m 2 / g.

[0013] Furthermore, the seed crystal contains SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.01-2.5:1, and the molar ratio of Na2O, H2O and SiO2 is 0.01-4.0:1.0-40.0:1; and / or the molar ratio of SiO2 to Al2O3 is 4.6-5.0:1, and the molar ratio of Na2O, H2O and SiO2 is 1.8-2.0:40-50:1.

[0014] Furthermore, the above-mentioned step S2 includes: step S21, gelling the aluminum-rich liquid and the silicon-rich liquid to obtain a first gel; step S22, aging the first gel and the seed crystal and performing a first hydrothermal crystallization treatment in sequence to obtain a 13X molecular sieve; wherein the first gel contains SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.5-6.0:1, and the molar ratio of Na2O, H2O and SiO2 is 0.5-6.0:10-100:1; preferably, the mass ratio of the seed crystal to the first gel is 5-20:100; and / or the aging treatment temperature is 20-100°C, and the aging treatment time is 0.1-24h; and / or the first hydrothermal crystallization treatment temperature is 60-105°C, and the first hydrothermal crystallization treatment time is 0.1-36h.

[0015] Furthermore, the preparation method further includes: a seed crystal preparation process, the preparation process including: stirring and mixing raw materials including an aluminum source, a second silicon source and water to obtain a second gel; adjusting the pH value of the second gel to 8.5-12.5 and then performing a second hydrothermal crystallization treatment to obtain a seed crystal; wherein the stirring and mixing rate is 200-800 rpm, and / or the stirring and mixing temperature is 20-100°C, and / or the stirring and mixing time is 0.1-24h; preferably, the pH value of the second gel is 11.8-12.2; preferably, the second silicon source is selected from any one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash, and white carbon black; preferably, the aluminum source is selected from any one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate. species; preferably, the second hydrothermal crystallization treatment includes a first hydrothermal crystallization treatment and a second hydrothermal crystallization treatment, wherein the temperature of the first hydrothermal crystallization treatment is 20-60°C, and / or the time of the first hydrothermal crystallization treatment is 4-24h; preferably, the temperature of the second hydrothermal crystallization treatment is 80-120°C, and / or the time of the second hydrothermal crystallization treatment is 6-48h; further, preferably, the temperature of the first hydrothermal crystallization treatment is 35-45°C, and / or the time of the first hydrothermal crystallization treatment is 11-13h; the temperature of the second hydrothermal crystallization treatment is 90-100°C, and / or the time of the second hydrothermal crystallization treatment is 22-26h; the temperature of the second hydrothermal crystallization treatment is 50-60°C higher than the temperature of the first hydrothermal crystallization treatment.

[0016] Furthermore, the preparation method further comprises a process of pretreating the waste molecular sieve, the pretreatment process comprising: sintering a mixture of the waste molecular sieve and the sodium salt to obtain a sintered product; using an acidic solution to sequentially perform aluminum dissolution treatment and solid-liquid separation on the sintered product to obtain an aluminum-rich liquid and a residue; using an alkaline solution to sequentially perform silicon dissolution treatment and solid-liquid separation on the residue to obtain a silicon-rich liquid; wherein the mass ratio of the waste molecular sieve to the sodium salt is 1:0.5-5; and / or the sintering temperature is 550-800°C, and / or the sintering time is 60-120min; and / or the acidic solution is a monobasic acid solution, and the mass fraction of the monobasic acid solution is 10-35%; preferably, the monobasic acid is hydrochloric acid and / or nitric acid; and / or the alkaline solution includes a monobasic alkali and water, and the mass ratio of the residue, the monobasic alkali and water is 1.5-100:40-60:50-400; and / or the monobasic alkali is NaOH and / or KOH; preferably, the waste molecular sieve is any one or more of waste Z-5 molecular sieve catalyst, waste MTO catalyst, waste molecular sieve adsorbent, fly ash, waste FCC catalyst, and waste VOC adsorbent; the sodium salt is Na2SO4 and / or NaCO3.

[0017] According to another aspect of the present invention, a VOCs adsorbent is provided. The VOCs adsorbent is prepared by the aforementioned preparation method.

[0018] Applying the technical solution of the present invention, steps S3 and S4 of the present application optimize the structure of the 13X molecular sieve to form a core-shell structure 13X molecular sieve with the 13X molecular sieve as the core, nickel nanoparticles as the intermediate layer, and titanium silicon molecular sieve as the shell. In this process, the 13X molecular sieve is sequentially subjected to a first impregnation treatment and a second impregnation treatment, and a nickel nanoparticle intermediate layer and a titanium silicon molecular sieve shell can be sequentially formed on the surface of the 13X molecular sieve to form a gradient structure, which helps to improve the mechanical strength and thermal stability of the molecular sieve. In this process, the structure of the 13X molecular sieve is greatly optimized, so that the resulting core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. The 13X molecular sieve with the core-shell structure is ion exchanged in step S5. The introduced cerium ions not only effectively increase the specific surface area and pore volume of the molecular sieve, significantly improve the adsorption capacity of the molecular sieve for VOCs, but also promote the formation of more active sites. The VOCs adsorbent obtained by the silanization modification treatment and the second calcination treatment of the calcined 13X molecular sieve in step S6 further enhances the adsorption performance of the VOCs adsorbent. In addition, the 13X molecular sieve prepared with waste catalyst as raw material in the present invention realizes waste utilization and reduces the cost of preparing the 13X molecular sieve. On the other hand, the VOCs adsorbent prepared by the method of the present application has excellent physical and chemical properties and environmental adaptability, and is suitable for environmental protection applications in multiple fields, especially industrial emissions and indoor air purification, and provides an efficient and environmentally friendly technical solution to the problem of VOCs pollution. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0020] As analyzed in the background technology of the present application, there are problems in the prior art of VOCs adsorbents with poor adsorption performance and low adsorption capacity. In order to solve this problem, the present application provides a VOCs adsorbent and a preparation method thereof.

[0021] In a typical embodiment of the present application, a method for preparing a VOCs adsorbent is provided, and the preparation method comprises the following steps: step S1, sequentially subjecting the waste molecular sieve to aluminum dissolution treatment and silicon dissolution treatment to obtain aluminum-rich liquid and silicon-rich liquid; step S2, sequentially subjecting the raw materials including the aluminum-rich liquid, the silicon-rich liquid and the seed to gelation treatment, aging treatment, and first hydrothermal crystallization treatment to obtain a 13X molecular sieve; step S3, sequentially subjecting the 13X molecular sieve to a first impregnation treatment and a second impregnation treatment in a silanization agent solution and a nickel-containing solution to obtain Nickel-modified 13X molecular sieve; step S4, subjecting a mixture including the nickel-modified 13X molecular sieve and a titanium silicon molecular sieve precursor solution to a first hydrothermal reaction and a roasting treatment in sequence to obtain a core-shell structure 13X molecular sieve; step S5, subjecting the cerium ion solution to an ion exchange reaction with the core-shell structure 13X molecular sieve, and then sequentially performing drying, alkaline solution treatment, and a first calcination treatment to obtain a calcined 13X molecular sieve; and step S6, sequentially performing a silanization modification treatment and a second calcination treatment on the calcined 13X molecular sieve to obtain a VOCs adsorbent.

[0022] Steps S3 and S4 of the present application optimize the structure of the 13X molecular sieve to form a core-shell structure 13X molecular sieve with the 13X molecular sieve as the core, nickel nanoparticles as the intermediate layer, and titanium silicon molecular sieve as the shell. In this process, the 13X molecular sieve is sequentially subjected to a first impregnation treatment and a second impregnation treatment, and a nickel nanoparticle intermediate layer and a titanium silicon molecular sieve shell can be sequentially formed on the surface of the 13X molecular sieve to form a gradient structure, which helps to improve the mechanical strength and thermal stability of the molecular sieve. In this process, the structure of the 13X molecular sieve is greatly optimized, so that the resulting core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. The 13X molecular sieve with the core-shell structure is ion exchanged in step S5. The introduced cerium ions not only effectively increase the specific surface area and pore volume of the molecular sieve, significantly improve the adsorption capacity of the molecular sieve for VOCs, but also promote the formation of more active sites. The VOCs adsorbent obtained by the silanization modification treatment and the second calcination treatment of the calcined 13X molecular sieve in step S6 further enhances the adsorption performance of the VOCs adsorbent. In addition, the 13X molecular sieve prepared with waste catalyst as raw material in the present invention realizes waste utilization and reduces the cost of preparing the 13X molecular sieve. On the other hand, the VOCs adsorbent prepared by the method of the present application has excellent physical and chemical properties and environmental adaptability, and is suitable for environmental protection applications in multiple fields, especially industrial emissions and indoor air purification, and provides an efficient and environmentally friendly technical solution to the problem of VOCs pollution.

[0023] In one embodiment of the present application, in the above step S3: the time of the first impregnation treatment is 8 to 24 hours; and / or the time of the second impregnation treatment is 24 to 48 hours; preferably, the molar concentration of the silanization agent solution is 0.05 to 0.2 mol / L; and / or the molar concentration of the nickel-containing solution is 0.05 to 0.2 mol / L; preferably, the volume ratio of the mass of the 13X molecular sieve to the silanization agent solution is 400 to 600:1 g / L; preferably, the nickel-containing solution is a nickel nitrate solution and / or a nickel sulfate solution; preferably, the silanization agent is selected from any one or more of 3-aminopropyltriethoxysilane, tetraethoxysilane and tetramethoxysilane;

[0024] It is preferred to control the time of the first impregnation treatment, the time of the second impregnation treatment, the molar concentration of the silanization agent solution and the molar concentration of the nickel-containing solution within the above ranges, which helps to control the quality of the nickel nanoparticles finally formed and improve the wetting effect of the silanization agent solution and the nickel-containing solution on the 13X molecular sieve; it is preferred to control the types of the nickel-containing solution and the silanization agent within the above ranges, which helps to enrich the selectivity of the nickel-containing solution and the silanization agent solution.

[0025] In one embodiment of the present application, the above-mentioned step S3 preferably also includes: subjecting the 13X molecular sieve obtained by the second impregnation treatment to a third calcination to obtain a nickel-modified 13X molecular sieve coated with a nickel nanoparticle layer; the atmosphere of the third calcination is preferably hydrogen, the temperature of the third calcination is 500-600°C, and the time of the third calcination is 2-4h.

[0026] The nickel compound attached to the surface of the 13X molecular sieve in the third calcination is decomposed at high temperature to form nickel oxide, and hydrogen reduces the nickel oxide to nickel nanoparticles. Preferably, controlling the temperature and time of the third calcination within the above range helps to improve the efficiency of forming nickel nanoparticles.

[0027] In one embodiment of the present application, in the above step S4, the temperature of the first hydrothermal reaction is 150-200°C, and the time of the first hydrothermal reaction is 12-24h; preferably, the temperature of the calcination treatment is 450-550°C, and the time of the calcination treatment is 4-8h; the titanium silicon molecular sieve precursor solution includes a first silicon source, a titanium source, a template, a fluorine complex and water, wherein the first silicon source, the titanium source, the template, the fluorine complex and the water are in a molar ratio of 1:0.04-0.1:0.1-0.3:0.03-0.06:2 0 to 50 mixing; preferably, the mass ratio of nickel-modified 13X molecular sieve to the volume ratio of titanium silicon molecular sieve precursor solution is 400 to 600:1 g / L; preferably, the first silicon source is selected from any one or more of SiO2, Na2SiO3 and Si(OC2H5)4; preferably, the titanium source is selected from any one or more of TiO2, TiCl4 and Na2TiO3; preferably, the fluorine complex is selected from any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate and ammonium fluoride; preferably, the template is an organic amine and / or a quaternary ammonium salt.

[0028] It is preferred to control the temperature and time of the first hydrothermal reaction within the above range, which helps to improve the interaction between the titanium silicon molecular sieve precursor and the nickel-modified 13X molecular sieve. It is preferred to control the temperature and time of the calcination treatment within the above range, which helps to improve the structural integrity of the core-shell structure 13X molecular sieve finally formed. It is preferred to control the molar ratio of the first silicon source, titanium source, template agent, fluorine complex and water within the above range, which helps to improve the uniformity of the pore size of the core-shell structure 13X molecular sieve. It is preferred to control the types of silicon source, titanium source, template agent and fluorine complex within the above range, which helps to improve the synergistic effect between the components, so that the coating layer formed on the surface of the 13X molecular sieve has higher stability.

[0029] In one embodiment of the present application, in the above step S5, the molar concentration of the cerium ion solution is 0.05-0.5 mol / L, calculated as the cerium ions in the cerium ion solution, and the mass and volume ratio of the core-shell structure 13X molecular sieve to the cerium ion solution is preferably 1-20:100 g / mL, and the cerium ion solution is preferably selected from any one or more of cerium chloride, cerium nitrate, cerium citrate, and cerium acetate; and / or the temperature of the ion exchange reaction is 45-60°C, and / or the time of the ion exchange reaction is 16-24h; the process of the alkaline solution treatment preferably includes: subjecting the dried molecular sieve to a third impregnation treatment in an alkaline solution, preferably the time of the third impregnation treatment is 1-3h, and preferably the alkaline solution is NaOH and / or KOH; preferably the first calcination treatment is carried out in an air atmosphere, preferably the temperature of the first calcination treatment is 400-600°C, and preferably the time of the first calcination treatment is 5-8h.

[0030] It is preferred to control the molar concentration of the cerium ion solution and the volume ratio of the mass of the core-shell structure 13X molecular sieve to the cerium ion solution within the above range, which helps to control the amount of cerium ions introduced into the core-shell structure 13X molecular sieve, thereby controlling the degree of modification of the core-shell structure 13X molecular sieve and the amount of active sites of the core-shell structure 13X molecular sieve. It is preferred that the temperature and time of the ion exchange reaction are within the above range to promote the rate of the ion exchange reaction, and the type of alkaline solution and the time for the third impregnation in the alkaline solution are within the above range, which helps to introduce mesopores and shorten the diffusion distance of molecules in the pores; it is preferred to control the temperature and time of the first calcination treatment in the air within the above range, which can improve the efficiency and effect of the first calcination treatment, thereby improving the adsorption performance and adsorption capacity of the VOCs adsorbent.

[0031] In one embodiment of the present application, in the above step S6, the time of the silanization modification treatment is 8 to 24 hours; preferably, the volume ratio of the silane reagent and the solvent is 1:5 to 10; preferably, the reagent used for the silanization modification treatment includes a silane reagent and a solvent; preferably, the silane reagent is selected from any one or more of methyltrimethoxysilane, ethyltriethoxysilane and propenyltrimethoxysilane; preferably, the solvent is selected from any one or more of ethanol, propanol and butanol; and / or the temperature of the second calcination treatment is 500 to 700°C, and the time of the second calcination treatment is 2 to 4 hours.

[0032] Carrying out silanization modification treatment within the above-mentioned silane reagent and solvent range can improve the hydrophobicity of the titanium silicon surface, thereby improving the adsorption performance and catalytic activity of the adsorbent; preferably controlling the temperature and time of the second calcination treatment within the above range can improve the efficiency and effect of the second calcination treatment.

[0033] In one embodiment of the present application, in the above step S2, the 13X molecular sieve contains silicon and aluminum, and the molar ratio of silicon to aluminum is 2.2 to 2.9:1; and / or the pore volume of the 13X molecular sieve is 0.3 to 0.5 cm 3 / g, and / or the specific surface area of ​​13X molecular sieve is 700-950m 2 / g.

[0034] Preferably, the prepared 13X molecular sieve has the above properties through steps S1 and S2 of the present application. Among them, the molar ratio of silicon element to aluminum element is preferably within the above range, which helps to improve the utilization rate of silicon source in 13X molecular sieve; the pore volume and specific surface area of ​​13X molecular sieve are preferably within the above range, which helps to provide more adsorption sites and is conducive to improving the circulation and diffusion performance of VOCs inside the molecular sieve.

[0035] In one embodiment of the present application, the above-mentioned seed crystals contain SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.01-2.5:1, and the molar ratio of Na2O, H2O and SiO2 is 0.01-4.0:1.0-40.0:1; and / or the molar ratio of SiO2 to Al2O3 is 4.6-5.0:1, and the molar ratio of Na2O, H2O and SiO2 is 1.8-2.0:40-50:1.

[0036] The above provides two seed crystals with different structures. It is preferred to control the molar ratio of SiO2 to Al2O3 and the molar ratio of Na2O, H2O and SiO2 within the above two ranges, respectively, to provide a variety of crystal nuclei for the formation of 13X molecular sieve, thereby helping to improve the formation of the 13X molecular sieve framework structure and improve the stability.

[0037] In one embodiment of the present application, the above-mentioned step S2 includes: step S21, gelling the aluminum-rich liquid and the silicon-rich liquid to obtain a first gel; step S22, aging the first gel and the seed crystal and performing a first hydrothermal crystallization treatment in sequence to obtain a 13X molecular sieve; wherein the first gel contains SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.5-6.0:1, and the molar ratio of Na2O, H2O and SiO2 is 0.5-6.0:10-100:1; preferably, the mass ratio of the seed crystal to the first gel is 5-20:100; and / or the aging treatment temperature is 20-100°C, and the aging treatment time is 0.1-24h; and / or the first hydrothermal crystallization treatment temperature is 60-105°C, and the first hydrothermal crystallization treatment time is 0.1-36h.

[0038] Furthermore, it is preferred that the aging process be carried out under stirring.

[0039] In order to promote the formation of 13X molecular sieve crystals, in one embodiment of the present application, it is preferred that the above-mentioned preparation method also includes a seed preparation process, and the preparation process includes: stirring and mixing raw materials including an aluminum source, a second silicon source and water to obtain a second gel; adjusting the pH value of the second gel to 8.5-12.5 and then performing a second hydrothermal crystallization treatment to obtain seed crystals; wherein the stirring and mixing rate is 200-800 rpm, and / or the stirring and mixing temperature is 20-100°C, and / or the stirring and mixing time is 0.1-24h; preferably, the pH value of the second gel is 11.8-12.2; further preferably, the pH value of the above-mentioned second gel is 12; preferably, the second silicon source is selected from any one or more of silica sol, tetraethyl orthosilicate, coarse-pore silica gel, silicon powder, fly ash, and white carbon black; preferably, the aluminum source is selected from any one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate.

[0040] In order to improve the crystallization degree of 13X molecular sieve, the second hydrothermal crystallization treatment preferably includes a first hydrothermal crystallization treatment and a second hydrothermal crystallization treatment, wherein the temperature of the first hydrothermal crystallization treatment is 20 to 60°C, and / or the time of the first hydrothermal crystallization treatment is 4 to 24 hours; the temperature of the second hydrothermal crystallization treatment is preferably 80 to 120°C, and / or the time of the second hydrothermal crystallization treatment is 6 to 48 hours; further, the temperature of the first hydrothermal crystallization treatment is preferably 35 to 45°C, and / or the time of the first hydrothermal crystallization treatment is preferably 60 to 80°C. The time of thermal crystallization treatment is 11 to 13 hours; the temperature of the second hydrothermal crystallization treatment is 90 to 100°C, and / or the time of the second hydrothermal crystallization treatment is 22 to 26 hours; the temperature of the second hydrothermal crystallization treatment is 50 to 60°C higher than the temperature of the first hydrothermal crystallization treatment; it is further preferred that the temperature of the first hydrothermal crystallization treatment is 40°C, and / or the time of the first hydrothermal crystallization treatment is 12 hours; the temperature of the second hydrothermal crystallization treatment is 95°C, and / or the time of the second hydrothermal crystallization treatment is 24 hours.

[0041] In addition, in order to further improve the mixing effect of the aluminum source, the silicon source and the water, the specific steps of stirring and mixing the raw materials of the aluminum source, the second silicon source and the water preferably include: stirring and mixing the silicon source and the water, the stirring and mixing temperature is 20 to 60°C, the stirring and mixing time is 0.1 to 12h, the stirring and mixing speed is 200 to 800rpm, and a silicon-containing solution is obtained, and the concentration of the silicon-containing solution is 28 to 99wt%; stirring and mixing the aluminum source and the water, the stirring and mixing temperature is 20 to 60°C, the stirring and mixing time is 0.1 to 12h, and the stirring and mixing speed is 200 to 800rpm, and an aluminum-containing solution is obtained, and the concentration of the aluminum-containing solution is 28 to 99wt%, and the silicon-containing solution and the aluminum-containing solution are stirred and mixed to obtain a second gel.

[0042] Preferably, the pH value of the second gel is adjusted by slowly adding a solid base or an aqueous base solution to the second gel; preferably, the base is selected from sodium hydroxide and / or potassium hydroxide.

[0043] Preferably, after the first hydrothermal crystallization treatment in step S22, the reaction product needs to be filtered and washed to neutrality, and then dried at 80-120° C. until there is no significant weight loss to obtain a 13X molecular sieve.

[0044] In order to remove impurities such as moisture and carbon deposits in the waste molecular sieve, and further reduce the preparation cost of 13X molecular sieve and increase the pore volume and specific surface area of ​​13X molecular sieve, in one embodiment of the present application, it is preferred that the above-mentioned preparation method also includes a process of pretreating the waste molecular sieve, and the pretreatment process includes: sintering a mixture including the waste molecular sieve and the sodium salt to obtain a sintered product; using an acidic solution to sequentially perform aluminum dissolution treatment and solid-liquid separation on the sintered product to obtain an aluminum-rich liquid and a residue; using an alkaline solution to sequentially perform silicon dissolution treatment and solid-liquid separation on the residue to obtain a silicon-rich liquid; wherein the mass ratio of the waste molecular sieve to the sodium salt is 1:0.5~5; and / or the temperature of the sintering treatment is The temperature is 550-800°C, and / or the sintering time is 60-120 min; and / or the acidic solution is a monobasic acid solution, and the mass fraction of the monobasic acid solution is 10-35%; preferably, the monobasic acid is hydrochloric acid and / or nitric acid; and / or the alkaline solution includes a monobasic alkali and water, and the mass ratio of the residue, the monobasic alkali and water is 1.5-100:40-60:50-400; and / or the monobasic alkali is NaOH and / or KOH; preferably, the waste molecular sieve is any one or more of waste Z-5 molecular sieve catalyst, waste MTO catalyst, waste molecular sieve adsorbent, fly ash, waste FCC catalyst, and waste VOC adsorbent; the sodium salt is Na2SO4 and / or NaCO3.

[0045] In addition, the size of the spent molecular sieve is preferably less than 200 mesh; and the preferred sodium salt is NaCO3.

[0046] In another typical embodiment of the present application, a VOCs adsorbent is provided. The VOCs adsorbent is prepared by the aforementioned preparation method.

[0047] The VOCs adsorbent obtained by the preparation method of the present application has high selectivity, high adsorption capacity, high diffusion performance and easy regeneration performance, and is suitable for environmental protection applications in multiple fields, especially industrial emissions and indoor air purification, and provides an efficient and environmentally friendly technical solution to the VOCs pollution problem.

[0048] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0049] Example 1

[0050] Preparation of 13X molecular sieve seed crystals: 21.0 g of silica sol (mass fraction of 30%) was dissolved in 36.0 g of deionized water, and pretreated in a closed reactor at 25°C for 1 hour to obtain a silicon-containing solution; 24 g of aluminum sulfate was dissolved in 18.0 g of deionized water, and stirred at 25°C for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution was slowly added dropwise to the silicon-containing solution, and the solution after the addition was stirred at 60°C for 8 hours to obtain a gel mixture; 6.74 g of sodium hydroxide was dissolved in 36 g of deionized water to obtain a sodium hydroxide aqueous solution. , adding sodium hydroxide aqueous solution to the gel mixture, controlling the pH value of the gel mixture to maintain at 12, obtaining a second gel, placing the second gel in a hydrothermal reactor, and performing two hydrothermal crystallization treatments, wherein the temperature of the first hydrothermal crystallization treatment is 40°C, the time of the first hydrothermal crystallization treatment is 12 hours, and the temperature of the second hydrothermal crystallization treatment is 95°C, the time of the second hydrothermal crystallization treatment is 24 hours, and a 13X molecular sieve seed solution is obtained, and the 13X molecular sieve seed solution is filtered, washed, and dried in sequence to obtain a 13X molecular sieve seed. The molar ratio of SiO2 to Al2O3 in the 13X molecular sieve seed is 1.5:1, and the molar ratio of Na2O, H2O to SiO2 is 1.6:32:1.

[0051] Preparation of 13X molecular sieve: The waste Z-5 molecular sieve catalyst is mixed with NaCO3 in a mass ratio of 1:2.5 for sintering treatment. The sintering temperature is 600°C and the sintering time is 100 min. The sintered product is then subjected to aluminum dissolution treatment with hydrochloric acid having a mass concentration of 25%, and then filtered to obtain aluminum-rich liquid and residue; the residue is mixed with NaOH and H2O in a mass ratio of 50:50:200 for silicon dissolution treatment, and then filtered to obtain silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a first gel; the above-mentioned 13X molecular sieve seed crystals and the first gel are mixed in a mass ratio of 10:100, and then aged and hydrothermally crystallized in sequence. The aging temperature is 50°C and the aging time is 12 h; the hydrothermal crystallization temperature is 70°C and the hydrothermal crystallization time is 24 h, and then dried to obtain 13X molecular sieve. The molar ratio of SiO2 to Al2O3 in the first gel is 3.5:1, the molar ratio of Na2O, H2O to SiO2 is 2.8:80:1, and the molar ratio of silicon to aluminum in the 13X molecular sieve is 2.60:1; the pore volume of the 13X molecular sieve is 0.4789 cm 3 / g, the specific surface area of ​​13X molecular sieve is 877.2m 2 / g.

[0052] Preparation of core-shell structure 13X molecular sieve: 300g of the above 13X molecular sieve powder is placed in 500mL of 0.2mol / L 3-aminopropyltriethoxysilane solution for a first impregnation treatment, and the first impregnation treatment time is 8 hours; then the treated 3X molecular sieve is placed in 500mL of 0.2mol / L nickel nitrate solution for a second impregnation treatment, and the second impregnation treatment time is 24 hours; the 13X molecular sieve after the second impregnation treatment is subjected to a third calcination in a hydrogen atmosphere at 500°C, and the third calcination time is 2 hours to obtain a nickel-modified 13X molecular sieve containing a nickel nanoparticle deposition layer, SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water are mixed to prepare A titanium silicon molecular sieve precursor solution is prepared, wherein the molar ratio of SiO2, TiO2, sodium hexafluorophosphate, sodium hexafluorophosphate and water is 1:0.06:0.15:0.04:40; 150 g of 13X molecular sieve containing a nickel nanoparticle deposition layer is added to 250 mL of the titanium silicon molecular sieve precursor solution, and after sufficient mixing, the mixture is transferred to a reactor for a first hydrothermal reaction at a temperature of 150°C and a time of 12 h; after the reaction is completed, the solid is taken out and washed with water, and then dried at 110°C for 12 hours, and the dried solid is calcined at a temperature of 450°C and a time of 4 h to obtain a core-shell structure 13X molecular sieve.

[0053] Preparation of VOCs adsorbent: 50g of 13X molecular sieve with core-shell structure was soaked in 250mL of 0.5mol / L cerium nitrate (Ce(NO3)3) solution for 24 hours of ion exchange reaction, and then the molecular sieve was dried at 110°C for 12 hours. The dried molecular sieve was soaked in a 2mol / L sodium hydroxide (NaOH) solution for 2 hours, and then calcined at 500°C in air for 6 hours. After that, the calcined molecular sieve was soaked in a mixed solution containing 50mL ethyltriethoxysilane (TEOS) and 450mL ethanol for 12 hours, and after drying, it was calcined at 600°C for 3 hours to form a VOCs adsorbent.

[0054] Example 2

[0055] The difference from Example 1 is that the preparation of 13X molecular sieve seed crystals is as follows: 1 g of silicon powder is dissolved in 18.0 g of deionized water, and after pretreatment at 25° C. for 1 hour in a closed reactor, a silicon-containing solution is obtained; 12 g of aluminum sulfate is dissolved in 18.0 g of deionized water, and stirred at 35° C. for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution is slowly added dropwise to the silicon-containing solution, and the solution after the addition is stirred at 50° C. for 6 hours to obtain a gel mixture; 2 g of sodium hydroxide is dissolved in 36 g of deionized water to obtain a sodium hydroxide aqueous solution, and the sodium hydroxide aqueous solution is added dropwise to the silicon-containing solution. Add to the gel mixture, control the pH value of the gel mixture to maintain at 11.8, obtain the second gel, place the second gel in a hydrothermal reactor, perform two hydrothermal crystallization treatments, the temperature of the first hydrothermal crystallization treatment is 50°C, the time of the first hydrothermal crystallization treatment is 14 hours, the temperature of the second hydrothermal crystallization treatment is 100°C, the time of the second hydrothermal crystallization treatment is 18 hours, obtain 13X molecular sieve seed solution, filter, wash and dry the 13X molecular sieve seed solution in turn to obtain 13X molecular sieve seeds, and finally obtain VOCs adsorbent. Among them, the molar ratio of SiO2 to Al2O3 of the 13X molecular sieve seeds is 0.6:1, the molar ratio of Na2O, H2O to SiO2 is 3:20:1, the silicon-aluminum ratio of the 13X molecular sieve is 2.40:1; the pore volume of the 13X molecular sieve is 0.4590cm 3 / g, the specific surface area of ​​13X molecular sieve is 873.2m 2 / g.

[0056] Example 3

[0057] The difference from Example 1 is that the preparation of 13X molecular sieve seed crystals is as follows: 0.17 g of silicon powder is dissolved in 6 g of deionized water, and pretreated in a closed reactor at 25°C for 1 hour to obtain a silicon-containing solution; 12 g of aluminum sulfate is dissolved in 18 g of deionized water, and stirred at 35°C for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution is slowly added dropwise to the silicon-containing solution, and the solution after the addition is stirred at 100°C for 24 hours to obtain a gel mixture; 0.9 g of sodium hydroxide is dissolved in 6 g of deionized water to obtain a sodium hydroxide aqueous solution, and the sodium hydroxide aqueous solution is added dropwise to the silicon-containing solution. Add to the gel mixture, control the pH value of the gel mixture to maintain at 12.5, obtain the second gel, place the second gel in a hydrothermal reactor, perform two hydrothermal crystallization treatments, the temperature of the first hydrothermal crystallization treatment is 60°C, the time of the first hydrothermal crystallization treatment is 24 hours, the temperature of the second hydrothermal crystallization treatment is 120°C, the time of the second hydrothermal crystallization treatment is 48 hours, obtain 13X molecular sieve seed solution, filter, wash and dry the 13X molecular sieve seed solution in turn to obtain 13X molecular sieve seeds, and finally obtain VOCs adsorbent. Among them, the molar ratio of SiO2 to Al2O3 of the 13X molecular sieve seeds is 0.1:1, the molar ratio of Na2O, H2O to SiO2 is 4:1:1, the silicon-aluminum ratio of the 13X molecular sieve is 2.23:1; the pore volume of the 13X molecular sieve is 0.3693cm 3 / g, the specific surface area of ​​13X molecular sieve is 801.2m 2 / g.

[0058] Example 4

[0059] The difference from Example 1 is that the preparation of 13X molecular sieve seed crystals is as follows: 14.65 g of tetraethyl orthosilicate is dissolved in 36.0 g of deionized water, and pretreated in a closed reactor at 25°C for 1 hour to obtain a silicon-containing solution; 12 g of aluminum sulfate is dissolved in 18.0 g of deionized water, and stirred at 35°C for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution is slowly added dropwise to the silicon-containing solution, and the solution after the addition is stirred at 20°C for 0.1 hour to obtain a gel mixture; 0.56 g of sodium hydroxide is dissolved in 6 g of deionized water to obtain a sodium hydroxide aqueous solution, and Sodium hydroxide aqueous solution is added to the gel mixture, and the pH value of the gel mixture is controlled to be maintained at 8.5 to obtain a second gel. The second gel is placed in a hydrothermal reactor and subjected to two hydrothermal crystallization treatments. The temperature of the first hydrothermal crystallization treatment is 20°C, and the time of the first hydrothermal crystallization treatment is 4 hours. The temperature of the second hydrothermal crystallization treatment is 80°C, and the time of the second hydrothermal crystallization treatment is 6 hours to obtain a 13X molecular sieve seed solution. The 13X molecular sieve seed solution is filtered, washed, and dried in sequence to obtain a 13X molecular sieve seed, and finally a VOCs adsorbent is obtained. Among them, the molar ratio of SiO2 to Al2O3 of the 13X molecular sieve seed is 2.5:1, the molar ratio of Na2O, H2O to SiO2 is .01:40:1, and the silicon-aluminum ratio of the 13X molecular sieve is 2.87:1; the pore volume of the 13X molecular sieve is 0.3916cm 3 / g, the specific surface area of ​​13X molecular sieve is 821.1m 2 / g.

[0060] Example 5

[0061] The difference from Example 1 is that the time of the first impregnation treatment is 24 hours, the time of the second impregnation treatment is 48 hours, the molar concentration of the silanization agent solution is 0.05 mol / L, the molar concentration of the nickel-containing solution is 0.05 mol / L, and finally a VOCs adsorbent is obtained.

[0062] Example 6

[0063] The difference from Example 1 is that the time of the first impregnation treatment is 7 hours, the time of the second impregnation treatment is 20 hours, the molar concentration of the silanization agent solution is 0.04 mol / L, the molar concentration of the nickel-containing solution is 0.04 mol / L, and finally a VOCs adsorbent is obtained.

[0064] Example 7

[0065] The difference from Example 1 is that the temperature of the third calcination is 600° C., the time of the third calcination is 4 hours, and a VOCs adsorbent is finally obtained.

[0066] Example 8

[0067] The difference from Example 1 is that the temperature of the third calcination is 400° C., the time of the third calcination is 1 hour, and a VOCs adsorbent is finally obtained.

[0068] Example 9

[0069] The difference from Example 1 is that the temperature of the first hydrothermal reaction is 200° C., the time of the first hydrothermal reaction is 24 h, the temperature of the calcination treatment is 550° C., the time of the calcination treatment is 8 h, and finally a VOCs adsorbent is obtained.

[0070] Example 10

[0071] The difference from Example 1 is that the temperature of the first hydrothermal reaction is 140° C., the time of the first hydrothermal reaction is 10 h, the temperature of the calcination treatment is 400° C., the time of the calcination treatment is 3 h, and finally a VOCs adsorbent is obtained.

[0072] Embodiment 11

[0073] The difference from Example 1 is that the molar ratio of SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water is 1:0.04:0.1:0.03:20, and a VOCs adsorbent is finally obtained.

[0074] Example 12

[0075] The difference from Example 1 is that the molar ratio of SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water is 1:0.1:0.3:0.06:50, and a VOCs adsorbent is finally obtained.

[0076] Example 13

[0077] The difference from Example 1 is that the molar ratio of SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water is 1:0.2:0.4:0.07:60, and a VOCs adsorbent is finally obtained.

[0078] Embodiment 14

[0079] The difference from Example 1 is that in the preparation of the VOCs adsorbent, 50 g of a core-shell structured 13X molecular sieve was immersed in 1000 mL of a 0.05 mol / L cerium chloride solution to carry out an ion exchange reaction, and finally a VOCs adsorbent was obtained.

[0080] Embodiment 15

[0081] The difference from Example 1 is that in the preparation of the VOCs adsorbent, 10 g of a core-shell structured 13X molecular sieve was soaked in 1000 mL of a 0.2 mol / L cerium chloride solution to carry out an ion exchange reaction, and finally a VOCs adsorbent was obtained.

[0082] Example 16

[0083] The difference from Example 1 is that in the preparation of the VOCs adsorbent, 10 g of a core-shell structured 13X molecular sieve was soaked in 1000 mL of a 0.5 mol / L cerium chloride solution to carry out an ion exchange reaction, and finally a VOCs adsorbent was obtained.

[0084] Embodiment 17

[0085] The difference from Example 1 is that in the preparation of the VOCs adsorbent, 10 g of a core-shell structured 13X molecular sieve was soaked in 1000 mL of a 0.02 mol / L cerium chloride solution to carry out an ion exchange reaction, and finally a VOCs adsorbent was obtained.

[0086] Embodiment 18

[0087] The difference from Example 1 is that in the preparation of the VOCs adsorbent, 10 g of a core-shell structured 13X molecular sieve was soaked in 1000 mL of a 0.6 mol / L cerium chloride solution to carry out an ion exchange reaction, and finally a VOCs adsorbent was obtained.

[0088] Comparative Example 1

[0089] The difference from Example 1 is that the 13X molecular sieve in step S2 is directly used as a VOCs adsorbent.

[0090] Comparative Example 2

[0091] The difference from Example 1 is that the core-shell structure 13X molecular sieve in step S4 is directly used as a VOCs adsorbent.

[0092] Comparative Example 3

[0093] The difference from Example 1 is that the core-shell structure 13X molecular sieve in step S4 is directly subjected to the treatment in step S6 to obtain a VOCs adsorbent.

[0094] Test Method

[0095] The 13X molecular sieve and VOCs adsorbent obtained in the above examples and comparative examples were structurally characterized and the adsorption performance of the VOCs adsorbent was tested. The results of the selectivity and adsorption efficiency of the VOCs adsorbent for VOCs are shown in Table 1.

[0096] The test methods for the silicon-to-aluminum ratio, pore capacity and specific surface area of ​​the 13X molecular sieve in Examples 1 to 4 are as follows:

[0097] The silicon-aluminum ratio of 13X molecular sieve is determined by X-ray fluorescence spectrometry (XRF);

[0098] Pore ​​capacity of 13X molecular sieve: BET test method;

[0099] Specific surface area of ​​13X molecular sieve: BET test method;

[0100] Adsorption performance of VOCs adsorbent: Fixed bed adsorption experiment: Take low-carbon alkanes such as ethane, ethylene, propylene (wherein the volume ratio of ethane, ethylene and propylene is 1:1:1) as the adsorption objects, pass them through a fixed bed containing adsorbent, and monitor the concentration changes through the bed layer. The adsorption capacity is determined by the weight of adsorbed VOCs (mg) / weight of adsorbent (g), and the unit is mg / g.

[0101] Table 1

[0102]

[0103] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0104] Steps S3 and S4 of the present application optimize the structure of the 13X molecular sieve to form a core-shell structure 13X molecular sieve with the 13X molecular sieve as the core, nickel nanoparticles as the intermediate layer, and titanium silicon molecular sieve as the shell. In this process, the 13X molecular sieve is sequentially subjected to a first impregnation treatment and a second impregnation treatment, and a nickel nanoparticle intermediate layer and a titanium silicon molecular sieve shell can be sequentially formed on the surface of the 13X molecular sieve to form a gradient structure, which helps to improve the mechanical strength and thermal stability of the molecular sieve. In this process, the structure of the 13X molecular sieve is greatly optimized, so that the resulting core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. The 13X molecular sieve with the core-shell structure is ion exchanged in step S5. The introduced cerium ions not only effectively increase the specific surface area and pore volume of the molecular sieve, significantly improve the adsorption capacity of the molecular sieve for VOCs, but also promote the formation of more active sites. The VOCs adsorbent obtained by the silanization modification treatment and the second calcination treatment of the calcined 13X molecular sieve in step S6 further enhances the adsorption performance of the VOCs adsorbent. In addition, the 13X molecular sieve prepared with waste catalyst as raw material in the present invention realizes waste utilization and reduces the cost of preparing the 13X molecular sieve. On the other hand, the VOCs adsorbent prepared by the method of the present application has excellent physical and chemical properties and environmental adaptability, and is suitable for environmental protection applications in multiple fields, especially industrial emissions and indoor air purification, and provides an efficient and environmentally friendly technical solution to the problem of VOCs pollution.

[0105] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a VOCs adsorbent, characterized in that: The preparation method comprises the following steps: Step S1, subjecting the waste molecular sieve to aluminum dissolution treatment and silicon dissolution treatment in sequence to obtain aluminum-rich liquid and silicon-rich liquid; Step S2, subjecting the raw materials including the aluminum-rich liquid, the silicon-rich liquid and the seed crystal to gelation treatment, aging treatment and first hydrothermal crystallization treatment in sequence to obtain 13X molecular sieve; Step S3, performing a first impregnation treatment and a second impregnation treatment on the 13X molecular sieve in a silanization agent solution and a nickel-containing solution in sequence to obtain a nickel-modified 13X molecular sieve; Step S4, subjecting the mixture including the nickel-modified 13X molecular sieve and the titanium silicon molecular sieve precursor solution to a first hydrothermal reaction and a calcination treatment in sequence to obtain a core-shell structure 13X molecular sieve; Step S5, subjecting the cerium ion solution to an ion exchange reaction with the core-shell structure 13X molecular sieve, followed by drying, alkaline solution treatment, and a first calcination treatment to obtain a calcined 13X molecular sieve; and Step S6, sequentially performing a silanization modification treatment and a second calcination treatment on the calcined 13X molecular sieve to obtain a VOCs adsorbent.

2. The preparation method according to claim 1, characterized in that: In step S3: The first immersion treatment time is 8 to 24 hours; and / or the second immersion treatment time is 24 to 48 hours; Preferably, the molar concentration of the silanization agent solution is 0.05-0.2 mol / L; and / or the molar concentration of the nickel-containing solution is 0.05-0.2 mol / L; preferably, the mass ratio of the 13X molecular sieve to the volume ratio of the silanization agent solution is 400-600:1 g / L; Preferably, the nickel-containing solution is a nickel nitrate solution and / or a nickel sulfate solution; Preferably, the silanization agent is selected from any one or more of 3-aminopropyltriethoxysilane, tetraethoxysilane and tetramethoxysilane; Preferably, step S3 further includes: The 13X molecular sieve obtained by the second impregnation treatment is subjected to a third calcination to obtain the nickel-modified 13X molecular sieve coated with a nickel nanoparticle layer; Preferably, the atmosphere of the third calcination is hydrogen, the temperature of the third calcination is 500-600° C., and the time of the third calcination is 2-4 hours.

3. The preparation method according to claim 1 or 2, characterized in that: In the step S4, The temperature of the first hydrothermal reaction is 150-200° C., and the time of the first hydrothermal reaction is 12-24 hours; Preferably, the calcination temperature is 450-550°C and the calcination time is 4-8h; The titanium silicon molecular sieve precursor solution comprises a first silicon source, a titanium source, a template, a fluorine complex and water, wherein the first silicon source, the titanium source, the template, the fluorine complex and the water are mixed in a molar ratio of 1:0.04-0.1:0.1-0.3:0.03-0.06:20-50; preferably, the mass ratio of the nickel-modified 13X molecular sieve to the volume ratio of the titanium silicon molecular sieve precursor solution is 400-600:1 g / L; Preferably, the first silicon source is selected from any one or more of SiO2, Na2SiO3 and Si(OC2H5)4; Preferably, the titanium source is selected from any one or more of TiO2, TiCl4 and Na2TiO3; Preferably, the fluorine complex is selected from any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate and ammonium fluoride; Preferably, the template is an organic amine and / or a quaternary ammonium salt.

4. The preparation method according to any one of claims 1 to 3, characterized in that In the step S5, the molar concentration of the cerium ion solution is 0.05-0.5 mol / L, based on the cerium ions in the cerium ion solution, and preferably the volume ratio of the mass of the core-shell structure 13X molecular sieve to the cerium ion solution is 1-20:100 g / mL, and preferably the cerium ion solution is selected from any one or more of cerium chloride, cerium nitrate, cerium citrate, and cerium acetate; and / or the temperature of the ion exchange reaction is 45-60° C., and / or the time of the ion exchange reaction is 16-24 h; Preferably, the alkaline solution treatment process comprises: performing a third impregnation treatment on the dried molecular sieve in an alkaline solution, preferably the time of the third impregnation treatment is 1 to 3 hours, and preferably the alkaline solution is NaOH and / or KOH; The first calcination treatment is preferably performed in an air atmosphere, the temperature of the first calcination treatment is preferably 400 to 600° C., and the time of the first calcination treatment is preferably 5 to 8 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S6, the silanization modification treatment time is 8 to 24 hours; Preferably, the reagent used for the silanization modification treatment includes a silane reagent and a solvent; preferably, the volume ratio of the silane reagent to the solvent is 1:5-10; preferably, the silane reagent is selected from any one or more of methyltrimethoxysilane, ethyltriethoxysilane and acryltrimethoxysilane; preferably, the solvent is selected from any one or more of ethanol, propanol and butanol; And / or the temperature of the second calcination treatment is 500-700° C., and the time of the second calcination treatment is 2-4 hours.

6. The preparation method according to any one of claims 1 to 5, characterized in that In step S2, the 13X molecular sieve contains silicon and aluminum, and the molar ratio of the silicon to the aluminum is 2.2 to 2.9:1; and / or the pore volume of the 13X molecular sieve is 0.3 to 0.5 cm 3 / g, and / or the specific surface area of ​​the 13X molecular sieve is 700-950m 2 / g.

7. The preparation method according to any one of claims 1 to 6, characterized in that The seed crystals contain SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of the SiO2 to the Al2O3 is 0.01-2.5:1, and the molar ratio of the Na2O, the H2O and the SiO2 is 0.01-4.0:1.0-40.0:1; And / or the molar ratio of the SiO2 to the Al2O3 is 4.6-5.0:1, and the molar ratio of the Na2O, the H2O and the SiO2 is 1.8-2.0:40-50:

1.

8. The preparation method according to any one of claims 1 to 7, characterized in that The step S2 comprises: Step S21, performing the gelation treatment on the aluminum-rich liquid and the silicon-rich liquid to obtain a first gel; Step S22, subjecting the first gel and the seed crystal to the aging treatment and the first hydrothermal crystallization treatment in sequence to obtain the 13X molecular sieve; wherein the first gel comprises SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of the SiO2 to the Al2O3 is 0.5-6.0:1, and the molar ratio of the Na2O, the H2O and the SiO2 is 0.5-6.0:10-100:1; Preferably, the mass ratio of the seed crystal to the first gel is 5 to 20:100; and / or the temperature of the aging treatment is 20 to 100°C, and the time of the aging treatment is 0.1 to 24 hours; and / or the temperature of the first hydrothermal crystallization treatment is 60 to 105°C, and the time of the first hydrothermal crystallization treatment is 0.1 to 36 hours.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method further comprises: The preparation process of the seed crystal comprises: Stirring and mixing raw materials including an aluminum source, a second silicon source and water to obtain a second gel; Adjusting the pH value of the second gel to 8.5-12.5 and then performing a second hydrothermal crystallization treatment to obtain the seed crystal; Wherein, the stirring and mixing speed is 200-800 rpm, and / or the stirring and mixing temperature is 20-100° C., and / or the stirring and mixing time is 0.1-24 h; Preferably, the pH value of the second gel is 11.8 to 12.2; Preferably, the second silicon source is selected from any one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash, and white carbon black; Preferably, the aluminum source is selected from any one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate; Preferably, the second hydrothermal crystallization treatment includes a first hydrothermal crystallization treatment and a second hydrothermal crystallization treatment, wherein: The temperature of the first hydrothermal crystallization treatment is 20 to 60° C., and / or the time of the first hydrothermal crystallization treatment is 4 to 24 hours; Preferably, the temperature of the second hydrothermal crystallization treatment is 80 to 120° C., and / or the time of the second hydrothermal crystallization treatment is 6 to 48 hours; Furthermore, it is preferred that the temperature of the first hydrothermal crystallization treatment is 35 to 45° C., and / or the time of the first hydrothermal crystallization treatment is 11 to 13 hours; The temperature of the second hydrothermal crystallization treatment is 90-100° C., and / or the time of the second hydrothermal crystallization treatment is 22-26 hours; The temperature of the second hydrothermal crystallization treatment is 50-60° C. higher than the temperature of the first hydrothermal crystallization treatment.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The preparation method further comprises a process of pretreating the waste molecular sieve, wherein the pretreatment process comprises: sintering a mixture of the waste molecular sieve and the sodium salt to obtain a sintered product; The sintered product is sequentially subjected to the aluminum dissolving treatment and solid-liquid separation using an acidic solution to obtain the aluminum-rich liquid and residue; Using an alkaline solution to sequentially perform the silicon dissolving treatment and solid-liquid separation on the residue to obtain the silicon-rich liquid; Wherein, the mass ratio of the waste molecular sieve to the sodium salt is 1:0.5-5; and / or the temperature of the sintering treatment is 550-800° C., and / or the time of the sintering treatment is 60-120 min; and / or the acidic solution is a monoprotic acid solution, the mass fraction of the monoprotic acid solution is 10-35%; preferably, the monoprotic acid is hydrochloric acid and / or nitric acid; and / or the alkaline solution comprises a monobasic alkali and water, the mass ratio of the residue, the monobasic alkali and the water is 1.5-100:40-60:50-400; and / or the monobasic alkali is NaOH and / or KOH; Preferably, the waste molecular sieve is selected from any one or more of waste Z-5 molecular sieve catalyst, waste MTO catalyst, waste molecular sieve adsorbent, fly ash, waste FCC catalyst, and waste VOC adsorbent; The sodium salt is Na2SO4 and / or NaCO3.

11. A VOCs adsorbent, characterized in that: The VOCs adsorbent is prepared by the preparation method described in any one of claims 1 to 10.

Citation Information

Patent Citations

  • Method for preparing molecular sieve from chlorosilane

    CN102009984A

  • Preparation method for efficiently synthesizing 13X-type molecular sieve from calcined kaolin by microwave-assisted hydrothermal method

    CN108726533A

  • Preparation method of high-dispersion rare earth oxide / SiO2 aerogel and application thereof

    CN112569897A

  • Method for modifying 13X molecular sieve for adsorbing VOCs

    CN113083227A

  • Method for synthesizing chemical grafting type solid amine adsorbent from FCC (fluid catalytic cracking) waste catalyst, obtained solid amine adsorbent and application of solid amine adsorbent

    CN115337899A