Preparation method of catalyst for improving stability and poisoning resistance of carrier
By using sonication and organic acids in catalyst preparation to promote the dispersion of Pt and support, the problems of low activity and ease of inactivation of conventional metal oxide catalysts are solved, and a catalyst that efficiently degrades Cl-VOCs is achieved, which significantly improves the catalytic oxidation performance and anti-chlorine poisoning properties.
Patent Information
- Application Number
- CN202410971230.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
Conventional metal oxide catalysts have low catalytic activity when degrading chlorine-containing organic compounds (Cl-VOCs) and are prone to inactivation, resulting in high energy consumption and secondary pollution problems.
A catalyst preparation method is adopted to improve the stability and anti-toxicity properties of the carrier. By mixing the Pt solution with organic acid and support powder, ultrasonic treatment and drying and forming, then grinding and calcining, forming an efficient Pt-based catalyst. The method includes sonication in the temperature range of 30-50°C and raising it to 400-600°C at a temperature increase rate of 5°C/min during the calcination process to improve the catalytic oxidation properties of the catalyst and anti-agglomeration ability.
Effectively improve the dispersion and binding capacity of Pt on the support surface, significantly improve the catalytic oxidation performance of the catalyst, and realize the low-temperature oxidation of Cl-VOCs. For example, the complete oxidation temperature of chlorobenzene is reduced to 335°C and the catalyst deactivation is reduced. risk.
Smart Images

Figure CN118925713A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preparation, and in particular to a method for preparing a catalyst with improved carrier stability and anti-poisoning performance. Background Art
[0002] Chlorinated organic compounds (Cl-VOCs) are volatile organic compounds with high toxicity, strong stability and poor reactivity. They are widely used in material synthesis, petroleum refining and drug production. Catalytic combustion technology is one of the effective means to purify Cl-VOCs pollutants, and the development of low-cost, high-efficiency, stable and broad-spectrum low-content precious metal catalysts is the key to realizing the application of this technology. Ca0, Al2O3, TiO2, SiO2 as cheap carriers not only have high temperature stability, but also have large specific surface area, regular pore structure, and contain rich acid sites. They are widely used in separation, adsorption and catalysis.
[0003] However, conventional metal oxides have low catalytic activity and produce more chlorine-containing byproducts during the catalytic degradation of Cl-VOCs, which in turn leads to higher energy consumption and secondary pollution. Currently, supported precious metal catalysts are still the mainstream catalysts for industrial applications due to their high activity and broad spectrum in the oxidative degradation of VOCs.
[0004] In order to effectively improve the catalytic activity of conventional metal oxides and reduce economic costs, a small amount of precious metals are usually loaded into metal oxides as active substances to improve their catalytic activity and the complete catalytic oxidation performance of the products. Precious metal Pt-based catalysts have been introduced into industrial applications due to their high catalytic activity, but their practical applications are limited by problems such as susceptibility to chlorine poisoning and agglomeration of active components leading to catalyst deactivation. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing a catalyst with improved carrier stability and anti-poisoning performance.
[0006] The present invention provides a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0007] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of an organic acid to completely dissolve it, and use a stirring rod to fully stir the solution during the dissolution process to form a uniform slurry;
[0008] Step 2: Ultrasonic treatment: 2 g of carrier powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 30-50° C.;
[0009] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried overnight to evaporate the water to obtain a formed dry solid;
[0010] Step 4: Grinding and calcining: The dried solid was ground into powder with the aid of an external grinding device, and transferred to a muffle furnace and heated to 400-600° C. at a heating rate of 5° C. / min and maintained for 4 h.
[0011] Preferably, other additives, such as phosphates, may be added during the mixing process to improve the structure and performance of the catalyst.
[0012] Preferably, the carrier mentioned in the ultrasonic treatment may be one of CaO, Al2O3, TiO2, and SiO2.
[0013] Preferably, the carrier Al2O3 needs to be pretreated before adding, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt.
[0014] Preferably, the organic acid mentioned in the mixing treatment may be one of tartaric acid, citric acid and oxalic acid.
[0015] Preferably, the ultrasonic time for promoting dispersion is 0.5-2 hours.
[0016] Preferably, the particle size of the dried solid after grinding is 30-50 mesh.
[0017] Beneficial effects of the present invention:
[0018] 1. The catalyst prepared by the present invention effectively improves the dispersibility and binding ability of Pt on the carrier surface, thereby effectively improving the catalytic oxidation performance and anti-agglomeration ability of the Pt-based catalyst, promoting the high dispersion and stability of active components such as precious metals, and enabling the supported catalyst to have good acidity and oxidizability, thereby realizing the low-temperature oxidation of industrially emitted VOCs.
[0019] 2. The catalyst prepared by the present invention uses an appropriate amount of organic acid to effectively promote the dispersion and stable binding of Pt on the carrier surface, which is beneficial to the dispersion and stabilization of Pt nanoparticles and improves the mass transfer properties of macromolecular reactants and products. In addition, the catalytic synergy between the abundant acid sites on the carrier surface and the highly dispersed Pt nanoparticle oxidation centers can significantly improve the low-temperature oxidation performance of the catalyst for pollutants. For example, the complete oxidation temperature of chlorobenzene (at a conversion rate of 99%) is only 335°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The Cl-VOCs degradation activities of Examples 1-3 and Comparative Example 1 are as follows: Figure 1 As shown;
[0021] Figure 2 The Cl-VOCs degradation activities of Examples 4-6 and Comparative Example 2 are as follows: Figure 2 shown. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0023] Example 1, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0024] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of citric acid to completely dissolve it, and use a stirring rod to fully stir it during the dissolution process to form a uniform slurry. During the mixing process, phosphate is added to improve the structure and performance of the catalyst;
[0025] Step 2: Ultrasonic treatment: 2 g of Al2O3 powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 30°C. The ultrasonic time for promoting dispersion is 0.5 hours. The carrier Al2O3 needs to be pretreated before addition, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt;
[0026] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0027] Step 4: Grinding and calcining: The dried solid was ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding was 30 mesh. After calcination, a 0.5Pt / Al2O3-N catalyst with a Pt loading of 0.5% was obtained.
[0028] Example 2, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0029] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of oxalic acid to completely dissolve it, and use a stirring rod to fully stir it during the dissolution process to form a uniform slurry. During the mixing process, phosphate is added to improve the structure and performance of the catalyst;
[0030] Step 2: Ultrasonic treatment: 2 g of Al2O3 powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 50°C. The ultrasonic time for promoting dispersion is 0.5 hours. The carrier Al2O3 needs to be pretreated before addition, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt;
[0031] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0032] Step 4: Grinding and calcining: The dried solid was ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding was 30 mesh. After calcination, a 0.5Pt / Al2O3-C catalyst with a Pt loading of 0.5% was obtained.
[0033] Example 3, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0034] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of tartaric acid to completely dissolve it, and use a stirring rod to fully stir it during the dissolution process to form a uniform slurry. During the mixing process, phosphate is added to improve the structure and performance of the catalyst;
[0035] Step 2: Ultrasonic treatment: 2 g of Al2O3 powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 40°C. The ultrasonic time for promoting dispersion is 0.5 hours. The carrier Al2O3 needs to be pretreated before addition, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt;
[0036] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0037] Step 4: Grinding and calcining: The dried solid is ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding is 30-50 mesh. After calcination, a 0.5Pt / Al2O3-J catalyst with a Pt loading of 0.5% is obtained.
[0038] Example 4, reference Figure 1-2, a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0039] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of citric acid to completely dissolve it, and use a stirring rod to fully stir it during the dissolution process to form a uniform slurry. During the mixing process, phosphate is added to improve the structure and performance of the catalyst;
[0040] Step 2: Ultrasonic treatment: 2 g of TiO2 powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 50° C. The ultrasonic time for promoting dispersion is 1 hour. The carrier TiO2 needs to be pretreated before addition, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt;
[0041] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0042] Step 4: Grinding and calcining: The dried solid is ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding is 30-50 mesh. After calcination, a 0.5Pt / TiO2-N catalyst with a Pt loading of 0.5% is obtained.
[0043] Example 5, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0044] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of oxalic acid to completely dissolve it, and use a stirring rod to fully stir it during the dissolution process to form a uniform slurry. During the mixing process, phosphate is added to improve the structure and performance of the catalyst;
[0045] Step 2: Ultrasonic treatment: 2 g of TiO2 powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 40° C. The ultrasonic time for promoting dispersion is 0.5 hours. The carrier TiO2 needs to be pretreated before addition, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt;
[0046] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0047] Step 4: Grinding and calcining: The dried solid is ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding is 30 mesh. After calcination, a 0.5Pt / TiO2-C catalyst with a Pt loading of 0.5% is obtained.
[0048] Example 6, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0049] Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of tartaric acid to completely dissolve it, and use a stirring rod to fully stir it during the dissolution process to form a uniform slurry. During the mixing process, phosphate is added to improve the structure and performance of the catalyst;
[0050] Step 2: Ultrasonic treatment: 2 g of TiO2 powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 50° C. The ultrasonic time for promoting dispersion is 0.5 hours. The carrier TiO2 needs to be pretreated before addition, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt;
[0051] Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0052] Step 4: Grinding and calcining: The dried solid is ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding is 30 mesh. After calcination, a 0.5Pt / TiO2-J catalyst with a Pt loading of 0.5% is obtained.
[0053] Comparative Example 1, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0054] Step 1: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 2 g of Al2O3 powder and perform ultrasonic treatment at a temperature range of 50°C, and the ultrasonic time for promoting dispersion is 0.5 hours;
[0055] Step 2: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0056] Step 3: Grinding and calcining: The dried solid was ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding was 30 mesh. After calcination, a 0.5Pt / Al2O3 catalyst with a Pt loading of 0.5% was obtained.
[0057] Comparative Example 2, reference Figure 1-2 , a method for preparing a catalyst with improved carrier stability and anti-poisoning performance, comprising the following preparation steps:
[0058] Step 1: Take 50 ml of a Pt solution having a Pt content of 200 mg / L, then add 2 g of TiO2 powder and perform ultrasonic treatment at a temperature range of 50° C. The ultrasonic time for promoting dispersion is 0.5 hours;
[0059] Step 2: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried for 12 hours to evaporate the water to obtain a formed dry solid;
[0060] Step 3: Grinding and calcining: The dried solid is ground into powder with the help of external grinding equipment, and transferred to a muffle furnace and heated to 500°C at a heating rate of 5°C / min and maintained for 4 hours. The particle size of the dried solid after grinding is 30 mesh. After calcination, a 0.5Pt / TiO2 catalyst with a Pt loading of 0.5% is obtained.
[0061] Figure 1 and Figure 2 0.5Pt / Al and 0.5Pt / Ti as well as various catalysts prepared by organic acid complexation were displayed. It can be seen that the catalyst prepared by adding organic acid to the precursor solution showed a lower chlorobenzene degradation temperature and resistance to chlorine poisoning, which indicates that the addition of organic acid effectively improves the stability and dispersibility of the combination of Pt and the carrier, thereby effectively promoting the improvement of Pt catalytic activity. Among them, the 0.5Pt / Al-C catalyst prepared with Al2O3 as the carrier and oxalic acid as the organic acid showed the best catalytic activity. It shows the advantages of this catalyst in the purification of Cl-VOCs.
[0062] Table 1 (Comparison of Cl-VOCs degradation T90 of Examples 1-6 and Comparative Examples 1-2 is shown in the following table:)
[0063]
[0064] Note: The catalyst mass is 100 mg, the particle size is 40-60 mesh, the chlorobenzene concentration is 500±50 ppm, and the mass space velocity is 30000 mL / (g*h).
[0065] Table 1 lists the T90 and T50 of chlorobenzene degradation by different catalysts prepared with Al2O3 and TiO2 carriers. The catalysts prepared by complexing Pt with different organic acids (Examples 1-6) have improved catalytic oxidation activity for chlorobenzene, effectively reducing the temperature of chlorobenzene conversion (conversion rate>90%). The lower the T90, the higher the oxidation activity of the catalyst; the catalysts prepared in Examples 1 and 2 have the highest oxidation activity, and the degradation T90 for chlorobenzene is only 334°C and 340°C. This shows that the catalysts prepared by this study can effectively degrade chlorobenzene and resist chlorine poisoning.
[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance, characterized in that: The method comprises the following preparation steps: Step 1: Mixing treatment: Take 50 ml of a Pt solution with a Pt content of 200 mg / L, then add 1 g of an organic acid to completely dissolve it, and use a stirring rod to fully stir the solution during the dissolution process to form a uniform slurry; Step 2: Ultrasonic treatment: 2 g of carrier powder is then added to the obtained slurry solution and ultrasonic treatment is performed at a temperature range of 30-50° C.; Step 3: Drying and forming: After the ultrasonic treatment is completed, the heterogeneous solution is transferred to an oven at 80°C and dried overnight to evaporate the water to obtain a formed dry solid; Step 4: Grinding and calcining: The dried solid was ground into powder with the aid of an external grinding device, and transferred to a muffle furnace and heated to 400-600° C. at a heating rate of 5° C. / min and maintained for 4 h.
2. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance according to claim 1, characterized in that: During the mixing process, other additives, such as phosphates, may be added to improve the structure and performance of the catalyst.
3. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance according to claim 1, characterized in that: The carrier mentioned in the ultrasonic treatment can be one of CaO, Al2O3, TiO2, and SiO2.
4. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance according to claim 3, characterized in that: The carrier Al2O3 needs to be pretreated before adding, such as calcination or acid washing, to improve its surface properties and facilitate the loading of Pt.
5. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance according to claim 1, characterized in that: The organic acid mentioned in the mixing treatment may be one of tartaric acid, citric acid and oxalic acid.
6. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance according to claim 1, characterized in that: The ultrasonic time for promoting dispersion is 0.5-2 hours.
7. A method for preparing a catalyst with improved carrier stability and anti-poisoning performance according to claim 1, characterized in that: The particle size of the dried solid after grinding is 30-50 mesh.
Citation Information
Patent Citations
Catalyst for removing chlorophenol compounds in water through low-temperature catalytic hydrogenation and preparation and application of catalyst
CN103691464A
Catalyst for efficient degradation of chlorine-containing organic waste gas at low temperature, preparation method and application thereof
CN111330606A
Pt catalyst and preparation method thereof
CN117443452A
Cited By
Preparation method, product and application of Cl-VOCs catalyst
CN120285988A