Method for preparing aluminum-based carrier with reduction function by using carbon-containing gas and method for preparing bimetallic monatomic catalyst
The carbon-containing gas heat treatment forms a reducing aluminum-based support, and directly reduces metal ions in situ, solving the problem of agglomeration of bimetal single atom catalyst under high temperature heat treatment, realizing the atomic morphological dispersion of bimetallic atoms, simplifying the preparation process and Improves catalytic activity.
Patent Information
- Application Number
- CN202411132378.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing bimetal single-atom catalyst preparation method, high-temperature heat treatment leads to agglomeration of metal atoms, making it difficult to accurately control the bimetals to be uniformly and stably dispersed on the support with atomic size, and are complex in operation and high cost, which limits catalytic activity and application.
The aluminum-based material is heat treated with carbon-containing gas to form a reducing substance as a carrier, and the metal ions are directly reduced in situ by impregnation method to achieve uniform dispersion of bimetals in atomic form, and avoid metal agglomeration caused by high-temperature hydrogen reduction.
实现了双金属单原子催化剂的高度分散,简化了制备过程,降低了成本,避免了金属催化活性组分的失活,提高了催化剂的整体性能。
Smart Images

Figure HDA0004998304120000011 
Figure HDA0004998304120000012 
Figure HDA0004998304120000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a method for preparing an aluminum-based carrier with a reducing function and a bimetallic single-atom catalyst by utilizing a carbon-containing gas. Background Art
[0002] Catalysts are widely used in industries such as chemical conversion, petroleum, energy, pharmaceuticals, and the environment, and play a vital role in the domestic economy, the global environment, and human well-being. Among them, heterogeneous catalysts have the advantages of easy functionalization, easy recycling, reusability, and simple preparation, which have attracted widespread attention. However, the heterogeneous catalysts used in industrial production are usually nanometal catalysts. In the reaction, only a small number of metal nanoparticles with suitable sizes or specific exposed crystal faces can be regarded as catalytic active sites, resulting in low utilization of metal atoms and waste of resources. Single-atom catalysts further reduce the size of metal nanoparticles to the atomic level and form uniform active sites, which can make full use of the catalytic active sites, thereby improving the reaction activity and metal atom utilization of the catalyst. However, the structure of single-metal atom catalysts is relatively simple, lacking in atomic cooperation, and it is difficult to achieve high activity for different catalytic reactions at the same time by simply regulating the type of central metal atoms, atomic coordination structure, and carrier structure. And because the surface energy of single-atom catalysts is high, single-atom aggregation often occurs during activation or reaction, limiting their ability to show greater catalytic activity.
[0003] Bimetallic single-atom catalysts overcome the structural uniformity of single-atom catalysts, and the diversity of adsorption and activation sites on the catalyst leads to different electron transfer pathways, providing more possibilities for catalytic reactions and improving the overall performance of the catalyst. Therefore, the construction of bimetallic single-atom catalysts with high synergistic effects has become a research hotspot in the field of catalysis. In Chinese patent CN114522682B, bimetallic nanoparticles supported on carbon carriers are prepared by impregnating carbon carriers with equal volumes of bimetallic N and M precursor solutions, calcining with inert gas, and reducing with hydrogen at high temperature. Carbon monoxide and halogen-containing substances are then reacted with the bimetallic, and the bimetallic is subjected to an in-situ atomic-level dispersed heat treatment reaction to obtain a bimetallic single-atom catalyst. In Chinese patent CN112023934B, a bimetallic precursor powder Cu / In@ZIF-8 is synthesized by a one-pot method, and then the copper-indium bimetallic single-atom catalyst is obtained by high-temperature pyrolysis under inert gas protection. Hu Wenbin et al. prepared Ni-NC as a nitrogen-doped carbon substrate by high-temperature pyrolysis in Dual Pt-Ni atoms dispersed on N-doped carbon nanostructure with novel (NiPt)-N4C2 configurations for synergistic electrocatalytic hydrogen evolution reaction [J]. Science China Materials, 2023, 66 (4): 1389-1397, and then deposited Pt on NC and Ni-NC samples by atomic layer deposition (ALD) technology to obtain Pt / Ni-NC bimetallic single atom catalysts. The above methods all have high-temperature heat treatment processes in the preparation of bimetallic catalysts, which easily lead to metal atom agglomeration and make it difficult to accurately control the uniform and stable dispersion of the bimetallic on the carrier at atomic size. In addition, some methods are complicated to operate and costly, which hinders the catalytic activity of bimetallic single atom catalysts and their further application.
[0004] In order to solve the problems existing in the above-mentioned preparation methods of bimetallic single-atom catalysts, it is necessary to improve the existing preparation technology. The support material is one of the most important factors affecting the performance of supported metal catalysts. It is crucial for adjusting the particle size and shape, chemical composition, exposing active sites, and forming synergistic effects at the metal-support interface. Aluminum-based supports widely used in industry, such as various crystalline phases of alumina, alumina doped with other oxides, molecular sieves, and aluminum-containing hydrotalcites, have special advantages such as easily regulated surface properties, adjustable microstructures, large reserves, low costs, and simple industrial preparation processes. However, the use of aluminum-based supports to load metals usually adopts high-temperature roasting or reduces metal precursors under the action of reducing agents, and the active components are easy to agglomerate to form particles, which cannot give full play to their catalytic activity. Therefore, it is necessary to modify the surface of the aluminum-based support, design an aluminum-based support with a surface reduction function, and control the bimetallic to be uniformly and stably dispersed on the support surface in atomic form through a simple, mild, and efficient method. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing an aluminum-based carrier with a reducing function by heat-treating an aluminum-based material with a carbon-containing gas, and using the aluminum-based carrier to load a bimetallic to prepare a highly dispersed bimetallic single-atom catalyst.
[0006] The method for preparing an aluminum-based carrier with a reducing function using a carbon-containing gas provided by the present invention is characterized in that a reducing substance is formed on the surface of an aluminum-based material by treating the aluminum-based material with a carbon-containing gas. During the process of loading the bimetallic by the impregnation method, the reducing substance can simultaneously react with two metal ions, and then the substance is separated from the carrier surface to form a vacancy. The generated vacancy can anchor the pair of metals to form an atomic pair, so that the bimetallic is uniformly and stably dispersed on the carrier surface in the form of atoms. The specific steps are as follows:
[0007] A. Place the aluminum-based material in a tube furnace and seal it. First, pass the balance gas through the deoxidizer into the tube furnace and check the airtightness of the device. Then pass the reaction gas through the deoxidizer equipped with 20-80g 401 manganese-based deoxidizer into the tube furnace. After passing the reaction gas for 10-30 minutes, start programming the temperature to heat the reactor. After the reaction is completed, cool it to room temperature, quickly take out the reduced aluminum-based carrier obtained after treatment, and seal it in a vacuum packaging bag for storage.
[0008] The aluminum-based material is one of pseudo-boehmite, lanthanum-doped pseudo-boehmite, silicon-doped pseudo-boehmite, phosphorus-doped pseudo-boehmite, aluminum hydroxide, ZSM5-molecular sieve, and MgAl-LDHs, preferably pseudo-boehmite and aluminum hydroxide.
[0009] The reaction gas is a mixture of a carbon-containing gas and a balance gas in a certain volume ratio. The carbon-containing gas is selected from at least one of CH4, C2H6, C2H4, C2H2, CO, CH3Cl, CH2Cl2, CHCl3, and CCl4, and preferably the carbon-containing gas is any one or more of CH4, C2H6, C2H4, C2H2, and CO. The volume percentage of the carbon-containing gas in the reaction gas is 1%-80%, and the rest is the balance gas, and preferably the volume percentage of the carbon-containing gas is 1-60%. The balance gas is nitrogen.
[0010] The deoxidation device is a drying tube added with 401 manganese-based deoxidizer, and the 401 manganese-based deoxidizer is a manganese-based metal oxide, which is used for deoxidation and purification of nitrogen and carbon-containing gas.
[0011] The conditions of the programmed temperature heating reactor are: gas flow rate of 1 mL / min-100 mL / min, preferably 20 mL / min-80 mL / min; heating rate of 1-100°C / min, preferably 5-10°C / min; reaction temperature of 200-1000°C, preferably 400-800°C; reaction time of 0.5-10h, preferably 2-6h.
[0012] B. Dissolve the soluble metal M salt and the soluble metal Pd salt in deionized water, and ultrasonicate for 5-10 minutes to fully dissolve them to obtain a bimetallic precursor solution containing M and Pd. Use the aluminum-based carrier obtained in step A as a carrier, add the bimetallic precursor solution containing M and Pd as an impregnation solution, add the impregnation solution under 40-90°C water bath conditions, and add a magnetic stirrer at a speed of 300-1000rmp. After the water in the solution is evaporated, put the evaporated sample into an oven at 40-90°C and dry it for 4-24h to obtain a bimetallic single atom catalyst.
[0013] The soluble metal M salt is one of HAuCl4, NaAuCl4, RuCl3, RuCl3·3H2O, H2PtCl4, H2PtCl6, K2PtCl4, K2PtCl6, Pt(NO3)2, [Pt(NH3)4]Cl2, Rh(CH3COO)3, Rh(NO3)3, H2IrCl6 and Na2IrCl6, preferably one of HAuCl4, RuCl3 and H2PtCl6. The soluble metal Pd salt is one of Na2PdCl4, Pd(NH3)2Cl2, Pd(NO3)2, Pd(CH3COO)2, preferably Na2PdCl4.
[0014] The mass percentage of the metal M and metal Pd loaded in the bimetallic single atom catalyst in the catalyst is 0.01%-20%, preferably 0.01%-10%. The mass ratio of the metal M and metal Pd loaded in the bimetallic single atom catalyst in the catalyst is 0.1-20, preferably 0.1-10.
[0015] The bimetallic single atom catalyst is expressed as xMyPd / ZT, wherein M and Pd represent active components, M is any one of Au, Ru, Rh, Pt, and Ir, preferably any one of Au, Ru, and Pt; x and y respectively represent the mass percentage of the prepared bimetallic single atom catalyst, and ZT represents an aluminum-based carrier.
[0016] The obtained aluminum-based support and bimetallic single-atom catalyst were characterized, and the results are as follows:
[0017] Figure 1 (a) and (b) are XRD patterns of the alumina supports prepared in Example 1 and Example 2, respectively. It can be seen from the figures that γ-alumina was prepared by this method.
[0018] Figure 2 (1), (2), and (3) are low-temperature nitrogen adsorption-desorption curves (a) and pore size distribution diagrams (b) of the alumina carriers prepared in Examples 1, 2, and 3, respectively. It can be seen from Figure (a) that the adsorption isotherm curve of the sample prepared by this method is type IV, indicating that the catalyst has a good mesoporous structure, and the hysteresis loop is H3 type, indicating that the alumina carriers prepared in Examples 1, 2, and 3 are all mesoporous structures and the pores are "wedge-shaped holes" formed by the accumulation of flaky particles; Figure (b) shows that the pore size of the alumina carrier prepared by this method is between 2-72nm, and the most probable pore sizes are approximately 3.8nm and 9.3nm, respectively.
[0019] Figure 3 (1) and (2) are low-temperature nitrogen adsorption-desorption curves (a) and pore size distribution diagrams (b) of the ZSM5-molecular sieve carrier and MgAl-LDOs carrier prepared in Examples 4 and 5, respectively. It can be seen from Figure (a) that the adsorption isotherm of the sample prepared by this method is type IV, indicating that the catalyst has a good mesoporous structure, and the hysteresis loop is H2 type, indicating that the ZSM5-molecular sieve carrier and MgAl-LDOs carrier prepared in Examples 4 and 5 are both "ink bottle-shaped" mesoporous structures; Figure (b) shows that the pore sizes of the ZSM5-molecular sieve carrier and MgAl-LDOs carrier prepared in Examples 4 and 5 are both between 2-57nm, and the most probable pore size is about 7.5nm.
[0020] Figure 4The TEM image and EDS-mapping image of 0.5% Pt1.0% Pd / Al2O3 prepared in Example 2 show that there are no agglomerated metal particles on the surface of the carrier, indicating that the two metals Pd and Pt are uniformly and highly dispersed on the carrier.
[0021] Figure 5 (a), (b), (c) and (d) are TEM images of the bimetallic single atom catalysts prepared in Examples 2, 3, 4 and 5, respectively. No particles were found in any of them, indicating that after the aluminum-based materials such as aluminum hydroxide, pseudo-boehmite, ZSM-5 molecular sieve and aluminum-containing hydrotalcite MgAl-LDHs were treated with carbon-containing gas, the loaded bimetallic materials were highly dispersed in the form of single atoms.
[0022] Figure 6 This is the HAADF-STEM image of 1.0%Ru0.5%Pd / ZSM5-molecular sieve prepared in Example 4. From the image, it can be seen that the two metals Pd and Ru are distributed on the ZSM5-molecular sieve carrier in the form of diatomic pairs.
[0023] Figure 7 The XRD diagrams of 0.5% Au0.5% Pd / Al2O3 prepared in Example 1, 0.5% Au / Al2O3 prepared in Comparative Example 1 and 0.5% Pd / Al2O3 prepared in Comparative Example 2 show that γ-alumina was successfully prepared by this method, and no characteristic diffraction peaks of metal particles were observed in the three catalysts, indicating that the metal particles loaded on these catalysts are relatively uniformly dispersed.
[0024] Figure 8 The XPS graph (a) of Au4f of 0.5%Au0.5%Pd / Al2O3 prepared in Example 1 and 0.5%Au / Al2O3 prepared in Comparative Example 1, and the XPS graph (b) of Pd3d of 0.5%Au0.5%Pd / Al2O3 prepared in Example 1 and 0.5%Pd / Al2O3 prepared in Comparative Example 2, it is estimated based on the binding energy position that the valence of Au in the prepared 0.5%Au0.5%Pd / Al2O3 is slightly lower than the valence of Au in 0.5%Au / Al2O3, and the valence of Pd in 0.5%Au0.5%Pd / Al2O3 is slightly higher than the valence of Pd in 0.5%Pd / Al2O3, indicating that there is interaction between Au and Pd atoms in this bimetallic catalyst, and the bimetal exists in the form of atomic pairs.
[0025] Beneficial effects of the present invention:
[0026] The present invention utilizes carbon-containing gas to heat-treat aluminum-based materials to obtain aluminum-based carriers with special reducing substances on their surfaces. The aluminum-based carriers with reducing substances on their surfaces are used to load bimetallic materials, and two metal ions can be directly reduced in situ during the impregnation process, achieving simultaneous completion of metal ion loading and reduction, and finally the two metals are dispersed on the carrier in the form of atomic pairs. Compared with the high-temperature hydrogen reduction method in the traditional impregnation method, this method is simple to operate and has mild conditions, and can avoid the agglomeration of metal atoms during high-temperature reduction in the traditional impregnation method, which leads to the inactivation of metal catalytic active components. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 (a) and (b) are XRD patterns of the alumina supports prepared for Example 1 and Example 2, respectively.
[0028] Figure 2 (1), (2), and (3) are low-temperature nitrogen adsorption-desorption curves (a) and pore size distribution diagrams (b) of the alumina supports prepared in Examples 1, 2, and 3, respectively.
[0029] Figure 3 (1) and (2) are low-temperature nitrogen adsorption-desorption curves (a) and pore size distribution diagrams (b) of the ZSM5-molecular sieve carrier and MgAl-LDOs carrier prepared in Examples 4 and 5, respectively.
[0030] Figure 4 TEM image and EDS-mapping image of 0.5% Pt1.0% Pd / Al2O3 prepared in Example 2.
[0031] Figure 5 (a), (b), (c) and (d) are TEM images of the bimetallic single atom catalysts prepared in Examples 2, 3, 4 and 5, respectively.
[0032] Figure 6 This is the HAADF-STEM image of 1.0%Ru0.5%Pd / ZSM5-molecular sieve prepared in Example 4.
[0033] Figure 7 These are the XRD patterns of 0.5% Au0.5% Pd / Al2O3 prepared in Example 1, 0.5% Au / Al2O3 prepared in Comparative Example 1, and 0.5% Pd / Al2O3 prepared in Comparative Example 2.
[0034] Figure 8 The XPS graph (a) is the Au4f graph of 0.5% Au0.5% Pd / Al2O3 prepared in Example 1 and 0.5% Au / Al2O3 prepared in Comparative Example 1, and the XPS graph (b) is the Pd3d graph of 0.5% Au0.5% Pd / Al2O3 prepared in Example 1 and 0.5% Pd / Al2O3 prepared in Comparative Example 2. DETAILED DESCRIPTION
[0035] In the following examples, the gas percentages are by volume.
[0036] Example 1
[0037] A. Weigh 4.0000g of pseudo-boehmite and place it in a porcelain boat, then seal it in a tubular furnace. First, pass nitrogen through a deoxidizing device equipped with 30g 401 manganese-based deoxidizer into the tubular furnace, and check the airtightness of the device. Then pass the reaction gas through the above deoxidizing device into the tubular furnace for 15 minutes. The reaction gas is selected with a gas ratio of 20% CH4 / 80% N2 (balance gas), and heat treatment is performed at 500℃, the heating rate is 5℃ / min, the gas flow rate is 80mL / min, and the reaction time is 6h. After the reaction is completed, cool the sample to room temperature in the reaction atmosphere and take it out to obtain a reducing alumina carrier, which is sealed and stored in a vacuum packaging bag.
[0038] B. Take 0.0173g NaAuCl4 and 0.0276g Na2PdCl4 and dissolve them in 15mL deionized water, and ultrasonicate for 6min to fully dissolve them to prepare NaAuCl4-Na2PdCl4 bimetallic precursor solution. Place 2.0000g of the alumina carrier obtained in step A in a 100mL beaker, add the prepared bimetallic precursor solution, heat in a water bath at 80℃, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into an oven at 80℃ to dry, and the mass percentage of Au and Pd in the obtained catalyst is 0.5%, expressed as 0.5%Au0.5%Pd / Al2O3.
[0039] Example 2
[0040] A. Weigh 4.0000g of aluminum hydroxide and place it in a porcelain boat, then seal it in a tubular furnace. First, pass nitrogen through a deoxidizing device equipped with 30g of 401 manganese-based deoxidizer into the tubular furnace, and check the airtightness of the device. Then pass the reaction gas through the above-mentioned deoxidizing device into the tubular furnace for 15 minutes. The reaction gas is selected with a gas ratio of 5% C2H2 / 5% CH4 / 90% N2 (balance gas), and heat treatment is performed at 600℃, the heating rate is 10℃ / min, the gas flow rate is 80mL / min, and the reaction time is 6h. After the reaction is completed, cool the sample to room temperature in the reaction atmosphere and take it out to obtain a reducing alumina carrier, which is sealed and stored in a vacuum packaging bag.
[0041] B. Take 0.0210g H2PtCl6 and 0.0552g Na2PdCl4 and dissolve them in 15mL deionized water. Ultrasonicate for 6min to fully dissolve them to prepare H2PtCl6-Na2PdCl4 bimetallic precursor solution. Place 2.0000g of the alumina carrier obtained in step A in a 100mL beaker, add the prepared bimetallic precursor solution, heat in a 70℃ water bath, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into a 70℃ oven to dry. The mass percentage of Pt and Pd in the obtained catalyst is 0.5%, expressed as 0.5%Pt1.0%Pd / Al2O3.
[0042] Example 3
[0043] A. Weigh 4.0000g of pseudo-boehmite and place it in a porcelain boat, then seal it in a tubular furnace. First, pass nitrogen through a deoxidizing device equipped with 30g 401 manganese-based deoxidizer into the tubular furnace, and check the airtightness of the device. Then pass the reaction gas through the above deoxidizing device into the tubular furnace for 15 minutes. The reaction gas is selected with a gas ratio of 40% CO / 60% N2 (balance gas), and heat treatment is performed at 500℃, the heating rate is 5℃ / min, the gas flow rate is 60mL / min, and the reaction time is 4h. After the reaction is completed, cool the sample to room temperature in the reaction atmosphere and take it out to obtain a reducing alumina carrier, which is sealed and stored in a vacuum packaging bag.
[0044] B. Take 0.0205g RuCl3 and 0.0276g Na2PdCl4 and dissolve them in 15mL deionized water, and ultrasonicate for 6min to fully dissolve them to prepare RuCl3-Na2PdCl4 bimetallic precursor solution. Place 2.0000g of the alumina carrier obtained in step A in a 100mL beaker, add the prepared bimetallic precursor solution, heat in a 70℃ water bath, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into a 70℃ oven to dry, and the mass percentage of Ru and Pd in the obtained catalyst is 0.5%, expressed as 0.5%Ru0.5%Pd / Al2O3.
[0045] Example 4
[0046] A. Weigh 4.0000g ZSM-5 molecular sieve and place it in a porcelain boat, then seal it in a tubular furnace. First, pass nitrogen through a deoxidizing device equipped with 30g401 manganese-based deoxidizer into the tubular furnace, and check the airtightness of the device. Then pass the reaction gas through the above-mentioned deoxidizing device into the tubular furnace for 15 minutes. The reaction gas is selected with a gas ratio of 20% CH4 / 80% N2 (balance gas), and heat treatment is performed at 800℃, the heating rate is 10℃ / min, the gas flow rate is 50mL / min, and the reaction time is 4h. After the reaction is completed, cool the sample to room temperature in the reaction atmosphere and take it out to obtain a reducible ZSM-5 molecular sieve carrier, which is sealed and stored in a vacuum packaging bag.
[0047] B. Take 0.0410g RuCl3 and 0.0276g Na2PdCl4 and dissolve them in 15mL deionized water, and ultrasonicate for 6min to fully dissolve them to prepare RuCl3-Na2PdCl4 bimetallic precursor solution. Place 2.0000g of the ZSM-5 molecular sieve carrier obtained in step A in a 100mL beaker, add the prepared bimetallic precursor solution, heat in a 70℃ water bath, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into a 70℃ oven and dry it. The mass percentage of Ru and Pd in the obtained catalyst is 0.5%, expressed as 1.0%Ru0.5%Pd / ZSM5-molecular sieve.
[0048] Example 5
[0049] A. Prepare MgAl-LDHs carrier using coprecipitation method. Dissolve 11.8631g Mg(NO3)2 and 8.5202g Al(NO3) in 100mL deionized water to obtain solution A, and dissolve 0.6000g NaOH and 3.1800g Na2CO3 in 100mL deionized water to obtain solution B. Add solution A and solution B dropwise into a reactor containing 100mL deionized water to control the pH of the system at 9.6±0.05. Then heat the reactor to 70℃ for 8h, centrifuge and wash until the supernatant pH=7.0 and further dry to obtain MgAl-LDHs. Take 4.000g MgAl-LDHs and place it in a porcelain boat, put it in a tubular furnace and seal it. First, pass nitrogen into the tubular furnace through a deoxidizer equipped with 30g 401 manganese-based deoxidizer, and check the airtightness of the device. The reaction gas is then passed through the above-mentioned deoxygenation device and introduced into a tube furnace for 15 minutes. The reaction gas is selected with a gas ratio of 25% C2H6 / 75% N2 (balance gas), and a heat treatment is performed at 800°C, a heating rate of 5°C / min, a gas flow rate of 60mL / min, and a reaction time of 4h. After the reaction is completed, the sample is cooled to room temperature in the reaction atmosphere and taken out to obtain a reducing MgAl-LDOs carrier, which is sealed and stored in a vacuum packaging bag.
[0050] B. Take 0.0173g NaAuCl4 and 0.0276g Na2PdCl4 and dissolve them in 15mL deionized water, and ultrasonicate for 6min to fully dissolve them to prepare NaAuCl4-Na2PdCl4 bimetallic precursor solution. Place 2.0000g of the MgAl-LDOs carrier obtained in step A in a 100mL beaker, add the prepared NaAuCl4-Na2PdCl4 bimetallic precursor solution, heat in a water bath at 80℃, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into an oven at 80℃ to dry. The mass percentage of Au and Pd in the obtained catalyst is 0.5%, expressed as 0.5%Au0.5%Pd / MgAl-LDOs.
[0051] Comparative Example 1
[0052] The same alumina carrier was prepared under the conditions of Example 1 to prepare 0.5% Au / Al2O3.
[0053] A. Weigh 4.0000g of pseudo-boehmite and place it in a porcelain boat, then seal it in a tubular furnace. First, pass nitrogen through a deoxidizing device equipped with 30g 401 manganese-based deoxidizer into the tubular furnace, and check the airtightness of the device. Then pass the reaction gas through the above deoxidizing device into the tubular furnace for 15 minutes. The reaction gas is selected with a gas ratio of 20% CH4 / 80% N2 (balance gas), and heat treatment is performed at 500℃, the heating rate is 5℃ / min, the gas flow rate is 80mL / min, and the reaction time is 6h. After the reaction is completed, cool the sample to room temperature in the reaction atmosphere and take it out to obtain a reducing alumina carrier, which is sealed and stored in a vacuum packaging bag.
[0054] B. Take 0.0173g NaAuCl4 and dissolve it in 15mL deionized water, and ultrasonicate it for 6min to fully dissolve it to prepare NaAuCl4 metal precursor solution. Put 2.0000g of the alumina carrier obtained in step A into a 100mL beaker, add the prepared NaAuCl4 metal precursor solution, heat it in a water bath at 80℃, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into an oven at 80℃ to dry, and the mass percentage of Au in the obtained catalyst is 0.5%, expressed as 0.5% Au / Al2O3.
[0055] Comparative Example 2
[0056] The same alumina carrier was prepared under the conditions of Example 1 to prepare 0.5% Pd / Al2O3.
[0057] A. Weigh 4.0000g of pseudo-boehmite and place it in a porcelain boat, then seal it in a tubular furnace. First, pass nitrogen through a deoxidizing device equipped with 30g 401 manganese-based deoxidizer into the tubular furnace, and check the airtightness of the device. Then pass the reaction gas through the above deoxidizing device into the tubular furnace for 15 minutes. The reaction gas is selected with a gas ratio of 20% CH4 / 80% N2 (balance gas), and heat treatment is performed at 500℃, the heating rate is 5℃ / min, the gas flow rate is 80mL / min, and the reaction time is 6h. After the reaction is completed, cool the sample to room temperature in the reaction atmosphere and take it out to obtain a reducing alumina carrier, which is sealed and stored in a vacuum packaging bag.
[0058] B. Take 0.0276g Na2PdCl4 and dissolve it in 15mL deionized water, and ultrasonicate it for 6 minutes to fully dissolve it to prepare a Na2PdCl4 metal precursor solution. Place 2.0000g of the alumina carrier obtained in step A in a 100mL beaker, add the prepared Na2PdCl4 metal precursor solution, heat it in a water bath at 80℃, and control the stirring speed at 500rmp. After the water in the solution is evaporated, put the evaporated sample into an oven at 80℃ to dry, and the mass percentage of Pd in the obtained catalyst is 0.5%, expressed as 0.5% Pd / Al2O3.
Claims
1. A method for preparing an aluminum-based carrier with a reducing function and a bimetallic single-atom catalyst using a carbon-containing gas, characterized in that Here are the steps: A. Place the aluminum-based material in a tube furnace, seal it, first pass the balance gas into the tube furnace through a deoxygenator, check the air tightness of the device, then pass the reaction gas into the tube furnace after passing through the deoxygenator, and after passing the reaction gas for 10-30 minutes, start programming the temperature to heat the reactor. After the reaction is completed, cool it to room temperature, quickly take out the reduced aluminum-based carrier obtained after the treatment, and seal it in a vacuum packaging bag for storage; The aluminum-based material is one of pseudo-boehmite, lanthanum-doped pseudo-boehmite, silicon-doped pseudo-boehmite, phosphorus-doped pseudo-boehmite, aluminum hydroxide, ZSM5-molecular sieve, and MgAl-LDHs; The reaction gas is a mixture of a carbon-containing gas and a balance gas, wherein the carbon-containing gas is selected from at least one of CH4, C2H6, C2H4, C2H2, CO, CH3Cl, CH2Cl2, CHCl3, and CCl4; The volume percentage of carbon-containing gas in the reaction gas is 1%-80%, and the rest is balance gas, which is nitrogen; The conditions of the programmed temperature heating reactor are: gas flow rate of 1 mL / min-100 mL / min, heating rate of 1-100° C. / min, reaction temperature of 200-1000° C., and reaction time of 0.5-10 h; B. Dissolve soluble metal M salt and soluble metal Pd salt in deionized water, and ultrasonicate for 5-10 minutes to fully dissolve them to obtain a bimetallic precursor solution containing M and Pd. Use the aluminum-based carrier obtained in step A as a carrier, add the bimetallic precursor solution containing M and Pd as an impregnation solution, add the impregnation solution under 40-90°C water bath conditions, and add a magnetic bar for stirring at a speed of 300-1000rmp. After the water in the solution is evaporated, put the evaporated sample into an oven at 40-90°C and dry it for 4-24h to obtain a bimetallic single atom catalyst; In step B, the soluble metal M salt is one of HAuCl4, NaAuCl4, RuCl3, RuCl3·3H2O, H2PtCl4, H2PtCl6, K2PtCl4, K2PtCl6, Pt(NO3)2, [Pt(NH3)4]Cl2, Rh(CH3COO)3, Rh(NO3)3, H2IrCl6 and Na2IrCl6, and the soluble metal Pd salt is one of Na2PdCl4, Pd(NH3)2Cl2, Pd(NO3)2 and Pd(CH3COO)2; The mass percentage of the metal M and metal Pd loaded on the obtained bimetallic single atom catalyst in the catalyst is 0.01%-20%, and the mass ratio of the metal M and metal Pd loaded on the bimetallic single atom catalyst in the catalyst is 0.1-20.
2. The method according to claim 1, characterized in that The deoxidation device described in step A is added with 401 manganese-based deoxidizer.
3. The method according to claim 1, characterized in that The prepared bimetallic single-atom catalyst is expressed as xMyPd / ZT; wherein M and Pd represent active components; M is any one of Au, Ru, Rh, Pt, and Ir; x and y represent the mass percentages of metal M and metal Pd in the catalyst, respectively, and x and y are both 0.01%-20%; ZT represents an aluminum-based carrier obtained by treatment with a carbon-containing gas.
4. The method according to claim 1, characterized in that: The carbon-containing gas is any one or more of CH4, C2H6, C2H4, C2H2, and CO.
5. The method according to claim 1, characterized in that The device used in the method includes two or three gas cylinders, one of which is a balance gas, and the other one or two are carbon-containing gases; the volume percentage of carbon-containing gas in the reaction gas entering the tubular furnace is 1%-60%, and the rest is nitrogen.
6. The method according to claim 1, characterized in that The device used in the method comprises a carbon-containing gas cylinder, a balance gas cylinder, a deoxygenation device, a reactor, and a tail gas collection bottle; wherein the carbon-containing gas cylinder and the balance gas cylinder are respectively connected to the deoxygenation device through a mass flow meter, the deoxygenation device is connected to the reactor through a gas path, pressure gauges are provided at the gas inlet and outlet of the reactor, and a tail gas collection bottle is provided after the reactor.
Citation Information
Patent Citations
Composite metal oxide loading active metal catalyst and preparation method thereof
CN106732567A
PdM monatomic alloy catalyst for acetylene selective hydrogenation reaction and preparation method of PdM monatomic alloy catalyst
CN115532269A
Method and device for preparing alumina carrier and catalyst with reduction function by using carbon-containing mixed gas
CN118105962A
Selective hydrogenation alkyne removal method for C2 fraction in light hydrocarbon cracking process
CN118108566A
Vehicle collected by reducing the amount of waste styrofoam fitted with dissolution tanks that can be crushed
KR1020220146753A