Desulfurization catalyst as well as preparation method and application thereof

By preparing lanthanum oxide-cobalt oxide composite catalyst with high specific surface area and multiple alkaline sites, the problem of difficulty and low efficiency of COS removal in blast furnace gas is solved, and the refined desulfurization of gas and source emission reduction is achieved.

CN118925733APending Publication Date: 2024-11-12WUHAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991006.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art has problems of difficulty and low removal efficiency in removing carbonylsulfur (COS) in blast furnace gas, especially the weak alkaline sites of bare lanthanum oxide, resulting in poor removal effect.

Method used

Using a composite catalyst containing lanthanum and cobalt, an oxidation with high specific surface area and multiple alkaline sites is prepared by preparing a mixed brine solution containing lanthanum salt and cobalt salt, adding an alkaline aqueous solution, and conducting hydrothermal reaction and calcining. Lanthanum-cobalt oxide composite catalyst.

Benefits of technology

This catalyst has excellent performance in removing COS, achieving refined desulfurization of coal gas, achieving source emission reduction targets, and avoiding corrosion to equipment and environment and damage to human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925733A_ABST
    Figure CN118925733A_ABST
Patent Text Reader

Abstract

The invention provides a desulfurization catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: preparing a mixed salt aqueous solution containing lanthanum salt and cobalt salt; preparing an alkaline aqueous solution containing hydroxide; under stirring, dropwise adding an alkaline aqueous solution into the mixed salt aqueous solution to obtain a turbid liquid with the pH value of 14, and continuously stirring the turbid liquid for 30-60 minutes; carrying out a hydrothermal reaction on the turbid liquid, and washing and drying a precipitate to obtain a precursor; and calcining the precursor to obtain the desulfurization catalyst. The desulfurization catalyst disclosed by the invention is a composite catalyst containing lanthanum oxide and cobalt oxide, and has a relatively large specific surface area and more alkaline sites, so that the desulfurization catalyst has a relatively high catalytic desulfurization effect. The desulfurization catalyst disclosed by the invention is applied to a reaction of adsorbing and removing carbonyl sulfide, shows more excellent desulfurization performance, can realize fine desulfurization of coal gas, achieves the target of source emission reduction, avoids corrosion of carbonyl sulfide to pipelines or equipment, and reduces environmental pollution and damage to human bodies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and more specifically, relates to a desulfurization catalyst and a preparation method and application thereof. Background Art

[0002] Blast furnace gas is a combustible gas produced as a byproduct of the blast furnace ironmaking process. It is characterized by low calorific value (about 3500kJ / Nm 3 ), with a large exhaust volume, it is an important secondary energy source. The main components of blast furnace gas are CO, CO2, N2, H2, CH4, and also contain sulfur components up to 200 mg / m 3 , among which sulfides are mainly carbonyl sulfide (COS), accounting for 72.7% of the total sulfur content. COS has a large bond energy, and breaking of chemical bonds requires more energy. Its physicochemical properties are stable, but it still has certain chemical activity. At the same time, COS is also weakly acidic and can react with a variety of alkaline solutions, but its acidity is weaker than that of H2S gas, so it is more difficult to remove. Improper emission of COS in blast furnace gas can cause damage to human health and the natural environment. However, due to the chemical stability of COS, the deep removal of COS is still a great challenge.

[0003] At present, the main methods for removing COS are divided into dry desulfurization and wet desulfurization. Adsorption, catalytic hydrolysis, catalytic oxidation, and hydrogenation conversion are commonly used dry desulfurization methods. The processing capacity of catalytic hydrolysis and hydrogenation catalysts is enhanced compared to adsorption, but a large amount of catalyst is still required. Therefore, the development of catalysts with greater processing capacity is one of the current research directions for carbonyl sulfide removal. Catalytic hydrolysis of COS has the advantages of low energy input, less waste, and efficient generation of H2S; the catalytic activity and adsorption capacity of the hydrolysis catalyst are both high, and COS can be removed in a short time.

[0004] Rare earth metals can increase the number of basic sites, pore volume and specific surface area, thereby improving the efficiency of the catalyst, so the rare earth metal lanthanum (La) was selected for research, but the basic sites of bare lanthanum oxide are weak and single, and the removal of carbonyl sulfide is not effective. Therefore, it is urgent to develop a lanthanum-containing catalyst with better desulfurization effect. Summary of the invention

[0005] The object of the present invention is to provide a desulfurization catalyst and a preparation method and application thereof. The desulfurization catalyst has a better effect in the catalytic removal of carbonyl sulfide, can achieve the clean desulfurization of coal gas, and achieve the goal of source emission reduction.

[0006] To achieve the above object, the first aspect of the present invention provides a method for preparing a desulfurization catalyst, comprising the following steps:

[0007] preparing a mixed brine solution containing a lanthanum salt and a cobalt salt;

[0008] preparing an alkaline aqueous solution containing a hydroxide;

[0009] Under stirring, the alkaline aqueous solution is added dropwise to the mixed saline solution to obtain a suspension with a pH of 14, and the suspension is stirred for 30 to 60 minutes;

[0010] The suspension is subjected to a hydrothermal reaction, and the precipitate is washed and dried to obtain a precursor;

[0011] The precursor is calcined to obtain a desulfurization catalyst.

[0012] Furthermore, in the mixed salt solution, the molar ratio of lanthanum to cobalt is 1:1 to 1:9.

[0013] Furthermore, in the mixed salt solution, the molar ratio of lanthanum to cobalt is 1:1.

[0014] Furthermore, the lanthanum salt is lanthanum nitrate, and the cobalt salt is at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride.

[0015] Furthermore, the concentration of the alkaline aqueous solution is 5-6 mol / L.

[0016] Furthermore, the hydroxide is at least one of sodium hydroxide and potassium hydroxide.

[0017] Furthermore, the temperature of the hydrothermal reaction is 160-200° C., and the time is 10-12 hours.

[0018] Furthermore, the calcination temperature is 400-600° C. and the calcination time is 2-5 hours.

[0019] The second aspect of the present invention provides a desulfurization catalyst obtained by any of the preparation methods described above.

[0020] The third aspect of the present invention provides use of a desulfurization catalyst in removing COS.

[0021] Compared with the prior art, the present invention has the following technical effects:

[0022] The preparation method of a desulfurization catalyst of the present invention comprises the following steps: dropping an alkaline aqueous solution into a mixed salt solution containing a lanthanum salt and a cobalt salt, and then sequentially performing hydrothermal reaction and calcination to obtain a composite catalyst containing lanthanum oxide and cobalt oxide. The preparation method of the present invention is simple, the preparation process conditions are controllable, and large-scale production can be carried out.

[0023] A desulfurization catalyst of the present invention is a composite catalyst containing lanthanum oxide and cobalt oxide. The composite catalyst has a larger specific surface area and more basic sites, so it has a higher catalytic desulfurization effect.

[0024] A desulfurization catalyst of the present invention is used in the reaction of removing carbonyl sulfide by adsorption, and shows more excellent desulfurization performance, can realize the desulfurization of coal gas, achieve the goal of reducing emissions at the source, avoid the corrosion of pipelines or equipment caused by carbonyl sulfide, and reduce environmental pollution and damage to the human body. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0026] Figure 1 This is a comparison chart of the activity evaluation of the desulfurization catalysts prepared in Examples 1 to 5 of the present invention and Comparative Examples 1 to 3;

[0027] Figure 2 The XRD diffraction spectra of the desulfurization catalysts prepared in Examples 1 and 5 of the present invention;

[0028] Figure 3 This is a comparison chart of the activity evaluation of the desulfurization catalysts prepared in Example 1 of the present invention and Comparative Example 1;

[0029] Figure 4 This is a comparison chart of the activity evaluation of the desulfurization catalysts prepared in Example 5 of the present invention and Comparative Example 1;

[0030] Figure 5 This is a comparison chart of the activity evaluation of the desulfurization catalysts prepared in Example 1 of the present invention and Comparative Example 2;

[0031] Figure 6 This is a comparison chart of the activity evaluation of the desulfurization catalysts prepared in Example 1 of the present invention and Comparative Example 3. DETAILED DESCRIPTION

[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0034] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the mass described in the description of the embodiments of the present invention may be μg, mg, g, kg, or other mass units known in the biochemical field.

[0035] The embodiment of the present invention provides a desulfurization catalyst and a preparation method thereof, comprising the following steps:

[0036] (1) preparing a mixed salt solution containing lanthanum salt and cobalt salt;

[0037] (2) preparing an alkaline aqueous solution containing a hydroxide;

[0038] (3) under stirring, the alkaline aqueous solution is added dropwise to the mixed saline solution to obtain a suspension with a pH of 14, and the suspension is stirred for 30 to 60 minutes;

[0039] (4) subjecting the suspension to a hydrothermal reaction, and washing and drying the precipitate to obtain a precursor;

[0040] (5) calcining the precursor to obtain a desulfurization catalyst.

[0041] In the above step (1), the molar ratio of lanthanum to cobalt in the mixed salt solution is 1:1 to 1:9. When the molar ratio of lanthanum to cobalt is within this range, a desulfurization catalyst with good catalytic performance can be obtained. Preferably, the molar ratio of lanthanum to cobalt in the mixed salt solution is 1:1, and the desulfurization effect of the prepared catalyst is the best.

[0042] Specifically, during the preparation process, the amount of lanthanum (La) added to the mixed brine solution can be kept unchanged, the ratio of lanthanum to cobalt can be changed, and the amount of cobalt (Co) added can be gradually reduced. For example, the ratio of La to Co is 1:1, 3:1, 5:1, 7:1, etc., so that the catalyst precursor can be synthesized smoothly and a catalyst with better desulfurization effect can be prepared.

[0043] Furthermore, the lanthanum salt of the embodiment of the present invention is lanthanum nitrate, and the cobalt salt is at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride.

[0044] In the above step (2), the concentration of the alkaline aqueous solution is 5 to 6 mol / L. The hydroxide in the embodiment of the present invention may be at least one of sodium hydroxide and potassium hydroxide.

[0045] In the above step (3), the embodiment of the present invention uses a rubber-tipped dropper to slowly drip the alkaline aqueous solution into the mixed salt solution at a rate of 1 drop / s-2 drops / s to ensure that a precipitate is uniformly generated in the mixed solution. The process gradually generates a precipitate. After the titration is completed, check whether the pH of the suspension is 14, and then continue to stir for 30-60 minutes to allow the suspension to fully react, so that the properties of the generated precipitate are more uniform, ensuring that the subsequent catalyst has good catalytic activity and stability.

[0046] In the above step (4), the temperature of the hydrothermal reaction in the embodiment of the present invention can be 160-200° C., and the time can be 10-12 hours. The precursor can be dried at 80-100° C. for 8-12 hours.

[0047] In the above step (5), the calcination temperature of the embodiment of the present invention can be 400-600° C. and the time can be 2-5 hours. The lanthanum oxide-cobalt oxide composite catalyst is obtained by calcination, and the calcination process helps to increase the specific surface area of ​​the catalyst, so that the basic sites on the catalyst surface are more and more evenly distributed and exposed, thereby improving the desulfurization effect of the prepared catalyst.

[0048] A desulfurization catalyst and a preparation method thereof according to an embodiment of the present invention are illustrated below by means of a plurality of specific embodiments.

[0049] Example 1

[0050] At room temperature (20-30°C), 2.2928 g of La(NO3)3·6H2O and 1.5645 g of Co(NO3)2·6H2O were weighed and dissolved in 7.5 ml of deionized water, and ultrasonicated for 5 min to uniformly dissolve to obtain a mixed solution A, in which the amount of metal ion La was 3.53 mmol;

[0051] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0052] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0053] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0054] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0055] The obtained crystalline fine powder is placed in a crucible, which is placed in a muffle furnace. The heating process is set to be programmed from room temperature to 500°C at a heating rate of 6.3°C / min, and then calcined at 500°C for 3h to finally obtain the desulfurization catalyst La-Co-1; (La-Co-1, where 1 represents the lanthanum-cobalt molar ratio of 1).

[0056] Example 2

[0057] At room temperature (20-30°C), 2.2928 g of La(NO3)3·6H2O and 0.5215 g of Co(NO3)2·6H2O were weighed and dissolved in 7.5 ml of deionized water, and ultrasonicated for 5 min to uniformly dissolve to obtain a mixed solution A, in which the amount of metal ion La was 3.53 mmol;

[0058] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0059] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0060] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0061] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0062] The obtained crystalline fine powder is placed in a crucible, which is then placed in a muffle furnace. The heating process is set to be programmed from room temperature to 500°C at a heating rate of 6.3°C / min, and then calcined at 500°C for 3h to finally obtain the desulfurization catalyst La-Co-3; (La-Co-3, where 3 represents the lanthanum-cobalt molar ratio of 3).

[0063] Example 3

[0064] At room temperature (20-30°C), 2.2928 g of La(NO3)3·6H2O and 0.3129 g of Co(NO3)2·6H2O were weighed and dissolved in 7.5 ml of deionized water, and ultrasonicated for 5 min to uniformly dissolve to obtain a mixed solution A, in which the amount of metal ion La was 3.53 mmol;

[0065] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0066] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0067] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0068] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0069] The obtained crystalline fine powder is placed in a crucible, which is then placed in a muffle furnace. The heating process is set to be programmed from room temperature to 500°C at a heating rate of 6.3°C / min, and then calcined at 500°C for 3h to finally obtain the desulfurization catalyst La-Co-5; (La-Co-5, where 5 represents the lanthanum-cobalt molar ratio of 5).

[0070] Example 4

[0071] At room temperature (20-30°C), 2.2928 g of La(NO3)3·6H2O and 0.2235 g of Co(NO3)2·6H2O were weighed and dissolved in 7.5 ml of deionized water, and ultrasonicated for 5 min to uniformly dissolve to obtain a mixed solution A, in which the amount of metal ion La was 3.53 mmol;

[0072] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0073] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0074] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0075] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0076] The obtained crystalline fine powder is placed in a crucible, which is then placed in a muffle furnace. The heating process is set to be programmed from room temperature to 500°C at a heating rate of 6.3°C / min, and then calcined at 500°C for 3h to finally obtain the desulfurization catalyst La-Co-7; (La-Co-7, where 7 represents the lanthanum-cobalt molar ratio of 7).

[0077] Example 5

[0078] At room temperature (20-30°C), 2.2928 g of La(NO3)3·6H2O and 0.1738 g of Co(NO3)2·6H2O were weighed and dissolved in 7.5 ml of deionized water, and ultrasonicated for 5 min to uniformly dissolve to obtain a mixed solution A, in which the amount of metal ion La was 3.53 mmol;

[0079] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0080] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0081] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0082] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0083] The obtained crystalline fine powder is placed in a crucible, which is placed in a muffle furnace. The heating process is set to be programmed from room temperature to 500°C at a heating rate of 6.3°C / min, and then calcined at 500°C for 3h to finally obtain the desulfurization catalyst La-Co-9; (La-Co-9, where 9 represents the lanthanum-cobalt molar ratio of 9).

[0084] Comparative Example 1

[0085] At room temperature (20-30°C), 2.2928 g of La(NO3)3·6H2O was weighed and dissolved in 7.5 ml of deionized water, and then ultrasonicated for 5 min to uniformly dissolve to obtain solution A, in which the amount of metal ion La was 3.53 mmol;

[0086] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0087] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0088] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0089] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0090] The obtained crystalline fine powder was placed in a crucible, which was placed in a muffle furnace. The temperature was set to rise from room temperature to 500°C at a rate of 6.3°C / min. The crucible was then calcined at 500°C for 3h to finally obtain the desulfurization catalyst La.

[0091] Comparative Example 2

[0092] At room temperature (20-30°C), 1.5645 g of Co(NO3)2·6H2O was weighed and dissolved in 7.5 ml of deionized water, and then ultrasonicated for 5 min to uniformly dissolve to obtain solution A, in which the amount of metal ion Co was 3.53 mmol;

[0093] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0094] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0095] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0096] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0097] The obtained crystalline fine powder was placed in a crucible, which was placed in a muffle furnace. The temperature was set to rise from room temperature to 500°C at a rate of 6.3°C / min. It was then calcined at 500°C for 3h to finally obtain the desulfurization catalyst Co.

[0098] Comparative Example 3

[0099] At room temperature (20-30°C), 2.3235 g of Ce(NO3)3·6H2O and 1.5645 g of Co(NO3)2·6H2O were weighed and dissolved in 7.5 ml of deionized water, and ultrasonicated for 5 min to uniformly dissolve to obtain a mixed solution A, in which the amount of metal ion Ce was 3.53 mmol;

[0100] Weigh 13.125 g of NaOH into a beaker, dissolve it in 52.5 ml of deionized water, and stir with a magnetic stirrer to completely dissolve it to obtain a mixed solution B, wherein the concentration of sodium hydroxide in solution B is 6 mol / L, which serves as a precipitant;

[0101] Under the condition of stirring at 1000 rpm, solution B was dripped into solution A at a speed of 1 drop / s. The pH of the solution was measured with a precision pH test paper to ensure that the pH of the solution was 14. Stirring was continued at 1000 rpm for 45 min to obtain a suspension.

[0102] The obtained suspension was placed into a 100 ml polytetrafluoroethylene liner, the liner was placed into a stainless steel reactor and pressed tightly, the reactor was placed into a homogeneous reactor preheated to 180°C, and the reaction was carried out for 12 hours. After the reaction was completed, the reactor was placed in clean water to cool down;

[0103] The product of the previous step was centrifuged and washed at a speed of 6000 rpm for 1 min, and the centrifugation was performed twice to obtain a preliminarily washed precipitate; the precipitate was filtered and washed with deionized water until it was neutral, and then placed in an oven and dried at 100°C for 12 h, and then taken out and ground and sieved to obtain a fine powder product;

[0104] The obtained crystalline fine powder was placed in a crucible, which was placed in a muffle furnace. The heating process was set to be programmed from room temperature to 500°C at a heating rate of 6.3°C / min, and then calcined at 500°C for 3h to finally obtain the desulfurization catalyst Ce-Co-1; (Ce-Co-1, where 1 represents the molar ratio of cerium to cobalt).

[0105] Desulfurization evaluation experiments were conducted on the desulfurization catalysts prepared in Examples 1-5 of the present invention and Comparative Examples 1-3:

[0106] The desulfurization catalyst was placed on a tablet press, maintained at a pressure of 15 MPa for 120 seconds, and then crushed into fine particles with a pestle, and then sieved with a sieve to obtain particles of 40 to 60 meshes to obtain catalyst particles;

[0107] Weigh 0.5 g of desulfurization catalyst particles, place them in a quartz tube with an inner diameter of 7 mm and an outer diameter of 10 mm, fill both ends of the quartz tube with quartz sand and quartz wool, and place the quartz tube with the desulfurization catalyst in a tube furnace for desulfurization evaluation;

[0108] 100 ml / min nitrogen was introduced to purge the desulfurization catalyst, the temperature of the tube furnace was raised to 100 °C, and the catalyst was purged under nitrogen atmosphere for 1 hour to remove moisture and other adsorbed impurities;

[0109] Raise the temperature of the tube furnace to 200°C and maintain the temperature inside the furnace;

[0110] Switch nitrogen to a COS / N2 mixed gas with a total mixed gas flow rate of 100 ml / min and a COS volume concentration of 1000 ppm in the mixed gas, so that the desulfurization catalyst and the gas are fully in contact in the quartz tube to achieve the purpose of desulfurization;

[0111] The COS concentration at the outlet was measured by a gas chromatograph (with the detector being FPD) to obtain a breakthrough adsorption curve. When the outlet COS concentration reached 10% of the inlet concentration, it was defined as breakthrough adsorption, which was also the effective adsorption time. At this time, the feed gas was stopped and the reaction was terminated.

[0112] The experimental results of desulfurization evaluation are as follows: Figure 1 , Figure 3-6 As shown. Figure 1 It can be seen that the La-Co composite desulfurization catalyst prepared in the embodiment of the present invention has a certain desulfurization efficiency when the molar ratio of La to Co is in the range of 1:1 to 1:9, but when the molar ratio of Co to La is 1:1, the La-Co-1 composite desulfurization catalyst has the best desulfurization effect on La. Figure 3 to Figure 4 It can be seen that within a certain range, the efficiency of the desulfurization catalyst increases with the increase of the amount of Co added; Figure 5 It can be seen that the desulfurization effect of sample Co in comparative example 2 is very weak, reaching breakthrough at 15 minutes; Figure 6 It can be seen that the desulfurization efficiency of sample Ce-Co-1 of Comparative Example 3 is significantly weaker than that of sample La-Co-1 of Example 1, and it reaches breakthrough in about 70 minutes, which indicates that the desulfurization effect of the La-Co-1 catalyst prepared in the embodiment of the present invention is significantly better than that of the Ce-Co-1 catalyst.

[0113] Figure 2 The X-ray diffraction analysis diagrams of the desulfurization catalysts synthesized in Examples 1 and 5 of the present invention, the diffraction peaks of LaO2CO3 (JCPDS 37-0804) crystals can be clearly observed in both samples; in Example 1, due to the increase in the amount of Co added, the crystal diffraction peaks of Co3O4 (JCPDS 65-3103) were observed.

[0114] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.

Claims

1. A method for preparing a desulfurization catalyst, characterized in that: The following steps are involved: preparing a mixed brine solution containing a lanthanum salt and a cobalt salt; preparing an alkaline aqueous solution containing a hydroxide; Under stirring, the alkaline aqueous solution is added dropwise to the mixed saline solution to obtain a suspension with a pH of 14, and the suspension is stirred for 30 to 60 minutes; The suspension is subjected to a hydrothermal reaction, and the precipitate is washed and dried to obtain a precursor; The precursor is calcined to obtain a desulfurization catalyst.

2. The method for preparing a desulfurization catalyst according to claim 1, characterized in that: In the mixed salt solution, the molar ratio of lanthanum to cobalt is 1:1 to 1:

9.

3. The method for preparing a desulfurization catalyst according to claim 2, characterized in that: In the mixed salt solution, the molar ratio of lanthanum to cobalt is 1:

1.

4. The method for preparing a desulfurization catalyst according to claim 2, characterized in that: The lanthanum salt is lanthanum nitrate, and the cobalt salt is at least one of cobalt nitrate, cobalt sulfate and cobalt chloride.

5. The method for preparing a desulfurization catalyst according to claim 1, characterized in that: The concentration of the alkaline aqueous solution is 5-6 mol / L.

6. The method for preparing a desulfurization catalyst according to claim 5, characterized in that: The hydroxide is at least one of sodium hydroxide and potassium hydroxide.

7. The method for preparing a desulfurization catalyst according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 160-200° C., and the time is 10-12 hours.

8. The method for preparing a desulfurization catalyst according to claim 1, characterized in that: The calcination temperature is 400-600° C. and the calcination time is 2-5 hours.

9. A desulfurization catalyst, characterized in that: The product is obtained by the preparation method described in any one of claims 1 to 8.

10. Use of the desulfurization catalyst according to claim 9 in removing COS.