ReS2 / Ba0. 5Sr0. 5TiO3 composite catalyst and application of piezoelectric electro-catalytic reduction of carbon dioxide

By preparing ReS2/Ba0.5Sr0.5TiO3 composite catalyst, using ultrasonic stirring and hydrothermal reaction, the problems of high cost, high pollution and poor light absorption performance in the existing technology were solved, and efficient and safe carbon dioxide reduction was achieved, which enhanced Photocatalytic activity and CO yield.

CN118925748AActive Publication Date: 2024-11-12CHANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410990365.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing piezoelectric photocatalysts have problems such as high cost, high pollution and poor light absorption performance during carbon dioxide reduction process, and sacrificial agents are often required to improve activity, but this increases the cost and environmental pollution risk.

Method used

Prepare ReS2/Ba0.5Sr0.5TiO3 composite catalyst, through ultrasonic stirring and hydrothermal reaction methods, combined with tight Z-shaped heterojunction, the electron-hole separation efficiency is improved, the photocatalytic activity and carbon dioxide reduction ability are enhanced, and the photocatalytic activity and carbon dioxide reduction ability are avoided. Use of sacrificial agents.

Benefits of technology

It realizes efficient, safe and low-cost carbon dioxide reduction, reduces experimental risks and contamination, improves photoresponsiveness and CO yield, and shows better piezoelectric photocatalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure HDA0004958700190000011
    Figure HDA0004958700190000011
  • Figure HDA0004958700190000012
    Figure HDA0004958700190000012
Patent Text Reader

Abstract

The invention belongs to application in the field of piezoelectric electro-catalytic reduction of carbon dioxide, and particularly relates to a ReS2 / Ba0. 5Sr0. 5TiO3 composite catalyst and application in piezoelectric electro-catalytic reduction of carbon dioxide. The preparation method comprises the following steps: firstly, preparing a gel precursor of Ba < 0.5 > Sr < 0.5 > TiO3, and calcining to obtain white Ba < 0.5 > Sr < 0.5 > TiO3; the preparation method comprises the following steps: synthesizing a black cocatalyst ReS2 through a hydrothermal reaction, and finally preparing the ReS2 / Ba0. 5Sr0. 5TiO3 composite catalyst by adopting a mechanical stirring and solvent evaporation method. The catalyst has more excellent piezoelectric electro-catalytic performance and rich reaction active sites, when the catalyst is applied to piezoelectric electro-catalytic reduction of carbon dioxide, under the synergistic effect of illumination and ultrasound, the stable and excellent carbon dioxide reduction capacity is shown, and the application of Ba0. 5Sr0. 5TiO3 in the field of piezoelectric electro-catalytic reduction of carbon dioxide is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of piezoelectric photocatalysis, and specifically relates to a ReS2 / Ba 0.5 Sr 0.5 TiO3 composite catalyst and its preparation method and application. Background Art

[0002] Excessive carbon dioxide emissions have caused irreversible damage to the global environment. Converting excess carbon dioxide into high-energy value-added fuels is an important way to achieve sustainable development of the environment and energy. Among the many methods, piezoelectric photocatalytic reduction of CO2 is undoubtedly one of the most effective and environmentally friendly ways. People have been committed to finding efficient visible light-driven photocatalysts. More than one hundred photocatalysts have been reported for carbon dioxide conversion. However, most of these photocatalysts show limited activity under visible light. Since visible light accounts for 43% of solar energy, the inefficient use of solar energy is a great limitation. However, the introduction of piezoelectricity can bend the band structure of the material by generating an internal electric field, thereby achieving rapid and effective separation of photogenerated electrons and holes. At present, in the application field of photocatalytic and piezoelectric photocatalytic reduction of carbon dioxide, there is a common situation of adding sacrificial agents such as TEOA, lactic acid, and triethanolamine. Indeed, the addition of sacrificial agents can greatly improve the overall carbon dioxide reduction performance by donating electrons or promoting electron-hole separation. However, on the one hand, the addition of sacrificial agents will increase the overall cost. If the catalytic time is too long, the sacrificial agent needs to be supplemented, which is not conducive to the subsequent large-scale application. On the other hand, the recovery and removal of sacrificial agents and the pollution of sacrificial agents to the environment are also a major problem, which will also increase the difficulty and cost of catalysis. Therefore, considering the above many invariants, the catalytic reduction of carbon dioxide by pure water without sacrificial agents is undoubtedly the best choice. It not only greatly reduces the overall experimental cost, but is also an environmentally friendly catalyst, which is conducive to ecological protection and promotes harmonious coexistence between man and ecology.

[0003] Barium strontium titanate (BST) is an important perovskite material with good piezoelectricity and high structural stability. It is an excellent material for piezoelectric photocatalytic reduction of carbon dioxide. Barium strontium titanate has a wide range of applications in sensors, capacitors, etc. ReS2 has been used in photocatalytic reduction of carbon dioxide occasionally, but its application in piezoelectric photocatalytic reduction of carbon dioxide is rare. Most of these examples are limited to the single aspect of photocatalysis. In order to further improve its performance, the coupling of piezoelectricity and photocatalysis is imperative. Therefore, it is very important to study the efficiency of barium strontium titanate in piezoelectric photocatalytic reduction of carbon dioxide. At the same time, while barium strontium titanate has excellent piezoelectricity, poor light absorption is a major shortcoming. Therefore, the present invention intentionally introduces a co-catalyst ReS2 with excellent light absorption performance, aiming to improve its light absorption ability and accelerate the transfer speed of electrons, thereby greatly improving the photocatalytic performance. Summary of the invention

[0004] The purpose of the present invention is to prepare a ReS2 / Ba 0.5 Sr 0.5 TiO3 composite catalyst is used for piezoelectric photocatalytic reduction of carbon dioxide, which has higher piezoelectric photocatalytic activity and carbon dioxide reduction ability than pure substances.

[0005] ReS2 / Ba prepared by the present invention 0.5 Sr 0.5 The TiO3 composite catalyst, the preparation method thereof comprises the following steps:

[0006] (1)Ba 0.5 Sr 0.5 Preparation of TiO3 catalyst:

[0007] Tetrabutyl titanate was added to anhydrous ethanol and stirred for 25 minutes, then BaCO3 and SrCO3 were added, ultrasonic treatment was performed for 90 minutes, and stirring was performed for 30 minutes to obtain solution A. Deionized water, HCl and anhydrous ethanol were mixed and stirred for 25 minutes to obtain solution B. Solution B was then added dropwise into solution A to obtain a mixed solution in a gel state, which was then vacuum dried overnight to obtain a xerogel barium strontium titanate precursor. BaCO3 was then prepared by a solid phase method. 0.5 Sr 0.5 TiO3, put a certain amount of precursor into a tube furnace, fully calcine, and obtain a white product Ba 0.5 Sr 0.5 TiO3. (BST for short)

[0008] Furthermore, the molar ratio of BaCO3 and SrCO3 is 1:1; the molar ratio of BaCO3 and tetrabutyl titanate is 1:2; and the volume ratio of deionized water, HCl and anhydrous ethanol is 10:3.3:50.

[0009] The calcination temperature in the tubular furnace is 800-900°C, and the calcination time is 6-10 hours.

[0010] (2) Preparation of ReS2 catalyst:

[0011] Add NH4ReO4 and thiourea to a certain amount of deionized water, ultrasonically treat for a period of time, and then stir for 1 hour. Then add the above mixed solution into a polytetrafluoroethylene-lined hydrothermal reactor and hydrothermally react at 240°C for 24 hours. After the reaction is completed, cool to room temperature, wash the obtained black reactant repeatedly with deionized water and ethanol, and then vacuum dry at 60°C overnight to finally obtain the black product ReS2. (RS for short)

[0012] Furthermore, the molar ratio of NH4ReO4 and thiourea is 2:9.

[0013] (3)ReS2 / Ba 0.5 Sr 0.5 Preparation of TiO3 composite catalyst:

[0014] ReS2 and Ba 0.5 Sr 0.5 TiO3 is dispersed in a certain amount of solvent, and ReS2 / Ba is obtained after ultrasonication, stirring, filtering, washing and drying. 0.5 Sr 0.5 TiO3 composite catalyst.

[0015] Furthermore, the added mass of ReS2 is Ba 0.5 Sr 0.5 5-15% of TiO3 mass.

[0016] Furthermore, the solvent includes deionized water.

[0017] Furthermore, the ultrasonic power is 240 W, and the time is 1 h; the stirring speed is 400 r / min, and the time is 24 h.

[0018] The ReS2 / Ba prepared by the above method 0.5 Sr 0.5 TiO3 composite catalyst is used for piezoelectric photocatalytic reduction of carbon dioxide. The specific application method is: ReS2 / Ba 0.5 Sr 0.5 The TiO3 composite catalyst is added into water and dispersed evenly by ultrasound. Then CO2 is introduced without adding any sacrificial agent. Finally, piezoelectric photocatalytic reduction of carbon dioxide is carried out under the conditions of ultrasound and light.

[0019] Furthermore, the ultrasonic power is 240W; and the light is sunlight.

[0020] Furthermore, the ReS2 / Ba 0.5 Sr 0.5 The dosage of the TiO3 composite catalyst in water is 1-5 mg / 20 mL (preferably 2 mg / 20 mL).

[0021] The beneficial effects of the present invention are:

[0022] (1) The present invention greatly reduces the temperature of solid-phase firing by preparing the precursor of barium strontium titanate, greatly reduces the risk of the experiment, and has the advantages of simple and safe preparation process. 0.5 Sr 0.5 Application of TiO3 and ReS2 in piezoelectric photocatalytic reduction of carbon dioxide.

[0023] (2) The catalyst material of the present invention has the advantages of simple preparation and compounding process, rapidity, safety, high efficiency, no pollution, low preparation cost, etc. The compounding method of simple mechanical stirring and solvent evaporation is simple and efficient, and the fully uniform compounding can be seen from the EDS element mapping diagram.

[0024] (3) The present invention aims to promote the addition of catalyst ReS2. The lower overpotential indicates that the composite catalyst shows a lower overpotential at the same current density and a better light response, indicating that it has better photocatalytic activity and ability. At the same time, the smaller Tafel slope also indicates the enhanced carbon dioxide reduction activity and the increased CO production rate. The present invention prepares a tightly bound Z-type heterojunction by a simple mechanical stirring and solvent evaporation method, improves the separation efficiency of electron-hole pairs, and thus enhances the overall carbon dioxide reduction activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The ReS2 / Ba synthesized in Example 1 0.5 Sr 0.5 Scanning electron microscope image of TiO3 composite catalyst;

[0026] Figure 2 ReS2 and Ba 0.5 Sr 0.5 SEM image and EDS element mapping of pure TiO3;

[0027] Figure 3 Is ReS2, Ba 0.5 Sr 0.5 XRD pattern of TiO3 catalyst;

[0028] Figure 4 Ba with different Ba and Sr ratios x Sr 1-x XRD pattern of TiO3 catalyst;

[0029] Figure 5 ReS2 / Ba synthesized in Example 1-5 0.5 Sr 0.5 XRD pattern of TiO3 composite catalyst;

[0030] Figure 6 is a performance diagram of the CO production rate of the catalyst synthesized in Examples 1-7 under piezoelectric and photoelectric combination conditions;

[0031] Figure 7 is a performance diagram of the CO production rate of the catalyst synthesized in Example 1-7 under the piezoelectric effect only;

[0032] Figure 8 is a performance diagram of the CO production rate of the catalyst synthesized in Example 1-7 under the action of light only;

[0033] Fig. 9 Yes 0.5 Sr 0.5 TiO3 and ReS2 / Ba prepared in Example 1 0.5 Sr 0.5 Electrochemical LSV diagram of TiO3 composite catalyst.

[0034] Fig.10 Yes 0.5 Sr 0.5 TiO3 and ReS2 / Ba prepared in Example 1 0.5 Sr 0.5 Electrochemical Tafel diagram of TiO3 composite catalyst.

[0035] Fig.11 Ba calcined at 700°C and 800°C 0.5 Sr 0.5 TiO3 XRD pattern.

[0036] Fig.12 Yes 0.5 Sr 0.5 TiO3, ReS2 and ReS2 / Ba 0.5 Sr 0.5 XPS spectrum of TiO3 composite catalyst.

[0037] Fig.13 Yes 0.5 Sr 0.5 Mechanism diagram of piezoelectric photocatalytic reduction of carbon dioxide by TiO3 and ReS2. DETAILED DESCRIPTION

[0038] The present invention is not limited to the following specific embodiments. A person skilled in the art can implement the present invention in various other specific embodiments according to the contents disclosed in the present invention, or any design structure and idea of ​​the present invention with simple changes or modifications shall fall within the protection scope of the present invention. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0039]

[0040] R: CO yield, unit: μmol / (g·h)

[0041] S: CO peak area in gas chromatograph

[0042] m: catalyst mass, unit: g

[0043] t: time, unit: h.

[0044] Example 1

[0045] (1) 13.89 ml of tetrabutyl titanate was added to 37.5 ml of anhydrous ethanol, stirred for 25 min, then 3.946 g of BaCO3 and 2.952 g of SrCO3 were added, ultrasonically treated for 90 min, and stirred for 30 min to obtain solution A. 10 ml of deionized water, 3.3 ml of HCl and 50 ml of anhydrous ethanol were mixed and stirred for 25 min to obtain solution B. Then 13.3 ml of solution B was added dropwise into solution A to obtain a mixed solution, which was then vacuum dried overnight to obtain a xerogel barium strontium titanate precursor. BaCO3 was then prepared by a solid phase method. 0.5 Sr 0.5 TiO3, a certain amount of precursor was placed in a tube furnace and calcined at 800℃ for 8h. After sufficient calcination, a white product Ba was obtained. 0.5 Sr 0.5 TiO3. (BST for short)

[0046] (2) Add 2mmolNH4ReO4 and 9mmolthiourea to 60ml of deionized water, ultrasonically treat for a period of time, and then stir for 1h. Then add the above mixed solution into a polytetrafluoroethylene-lined hydrothermal reactor and hydrothermally react at 240℃ for 24h. After the reaction is completed, cool to room temperature, wash the obtained black reactant repeatedly with deionized water and ethanol, and then vacuum dry at 60℃ overnight to finally obtain the black product ReS2. (abbreviated as RS)

[0047] (3) ReS2 and Ba 0.5 Sr 0.5TiO3 was dispersed in deionized water, and then ultrasonicated (ultrasonic power was 240W, ultrasonic time was 1h), stirred (stirring speed was 400r / min, stirring time was 24h), filtered, washed, and dried to obtain a gray composite catalyst. 0.5 Sr 0.5 TiO3 composite catalyst; wherein the mass of ReS2 is ReS2 / Ba 0.5 Sr 0.5 10% of the mass of TiO3 composite catalyst was added with ReS2 and Ba 0.5 Sr 0.5 TiO3.

[0048] (4) The 10% ReS2 / Ba prepared in Example 1 0.5 Sr 0.5 TiO3 composite catalyst is used for piezoelectric photocatalytic reduction of carbon dioxide.

[0049] Put 2mg 10%ReS2 / Ba 0.5 Sr 0.5 The TiO3 composite catalyst was added to 20 ml of water and dispersed evenly by ultrasound. Without adding any sacrificial agent, CO2 was then introduced for 30 min, and finally the reaction was carried out in a closed state for 2 h under ultrasound (240 W) and light (55 W xenon lamp simulated sunlight). After the experiment, the gas in 0.5 mL of the tube was extracted, the peak area was detected by gas chromatograph, and the CO yield was calculated to be 23.80 μmol / (g·h).

[0050] Example 2

[0051] Compared with Example 1, the difference is that the mass of the co-catalyst ReS2 added in step (3) is ReS2 / Ba 0.5 Sr 0.5 5% of the mass of the TiO3 composite catalyst. Other experimental conditions are the same as those in Example 1. 0.5 Sr 0.5 TiO3.

[0052] The 5% ReS2-Ba prepared in Example 2 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 9.65 μmol / (g·h).

[0053] Example 3

[0054] Compared with Example 1, the difference is that the mass of the co-catalyst ReS2 added in step (3) is ReS2 / Ba 0.5 Sr 0.5The mass of the TiO3 composite catalyst is 7.5%. Other experimental conditions are the same as those in Example 1. It is recorded as 7.5% ReS2-Ba 0.5 Sr 0.5 TiO3.

[0055] The 7.5% ReS2-Ba prepared in Example 3 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 13.58 μmol / (g·h).

[0056] Example 4

[0057] Compared with Example 1, the difference is that the mass of the co-catalyst ReS2 added in step (3) is ReS2 / Ba 0.5 Sr 0.5 The mass of the TiO3 composite catalyst is 12.5%. Other experimental conditions are the same as those in Example 1. It is recorded as 12.5% ​​ReS2-Ba 0.5 Sr 0.5 TiO3.

[0058] The 12.5% ​​ReS2-Ba prepared in Example 4 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 9.19 μmol / (g·h).

[0059] Example 5

[0060] Compared with Example 1, the difference is that the mass of the co-catalyst ReS2 added in step (3) is ReS2 / B a0.5 Sr 0.5 The mass of the TiO3 composite catalyst is 15%. Other experimental conditions are the same as those in Example 1. 0.5 Sr 0.5 TiO3.

[0061] The 15% ReS2-Ba prepared in Example 5 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 4.38 μmol / (g·h).

[0062] Example 6

[0063] The catalyst of Example 6 is pure substance Ba 0.5 Sr 0.5 TiO3. The preparation method is the same as step (1) of Example 1.

[0064] The pure substance Ba of Example 6 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The other experimental conditions were consistent with those in Example 1, and the CO yield was 2.29 μmol / (g·h).

[0065] Example 7

[0066] The catalyst of Example 7 is pure ReS2. The preparation method is the same as step (2) of Example 1.

[0067] The pure substance ReS2 of Example 7 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those of Example 1, and the CO yield was 2.81 μmol / (g·h).

[0068] Comparative Example 1

[0069] Compared with Example 1-7, the catalyst is the same, the difference is that the experimental conditions of the piezoelectric photocatalytic hydrogen production experiment are changed from the synergistic conditions of ultrasound (240W) and light (55W xenon lamp simulated sunlight) to ultrasound (240W) only. Other experimental conditions are the same as those of Example 1-7. The measured CO yield is shown in Figure 7 .

[0070] Comparative Example 2

[0071] Compared with Example 1-7, the catalyst is the same, the difference is that the experimental conditions of the piezoelectric photocatalytic hydrogen production experiment are changed from the synergistic conditions of ultrasound (240W) and light (55W xenon lamp simulated sunlight) to the catalytic reaction under the condition of light (55W xenon lamp simulated sunlight). Other experimental conditions are the same as those of Example 1-7. The measured CO yield is shown in Figure 8 .

[0072] Comparative Example 3

[0073] Compared with Example 1, the difference is that in step (4), the amount of catalyst in the piezoelectric photohydrogen production experiment is changed from 2 mg to 1 mg, and the other conditions are consistent with Example 1, and the CO yield rate is 16.57 μmol / (g·h).

[0074] Comparative Example 4

[0075] Compared with Example 1, the difference is that in step (4), the amount of catalyst in the piezoelectric photohydrogen production experiment is changed from 2 mg to 3 mg, and the other conditions are consistent with Example 1, and the CO yield rate is 4.89 μmol / (g·h).

[0076] Comparative Example 5

[0077] Compared with Example 1, the difference is that in step (4), the amount of catalyst in the piezoelectric photohydrogen production experiment is changed from 2 mg to 5 mg, and the other conditions are consistent with Example 1, and the CO yield rate is 3.90 μmol / (g·h).

[0078] The other experimental conditions remain unchanged. As the amount of catalyst added increases, there will be mutual shielding between the catalysts, resulting in poor light absorption and reduced piezoelectric influence. At the same time, the active sites of the actual reaction are reduced. Therefore, adding too much catalyst will reduce the overall reaction rate and is not conducive to the piezoelectric photocatalytic reduction of carbon dioxide.

[0079] Comparative Example 6

[0080] Compared with Example 1, the difference is that in step (3), the composite solvent is changed from deionized water to ethanol, and the other conditions are consistent with Example 1, and the CO yield rate is 6.32 μmol / (g·h).

[0081] Compared with ethanol, the catalyst has better dispersibility in water and better composite effect. After the composite is completed, the composite with water as the solvent only needs to be left for a while, and the composite can be deposited at the bottom, which is easier to separate from the water and is conducive to subsequent drying. However, the composite with ethanol as the solvent will not be deposited to the bottom no matter how long it is left, which will affect the subsequent drying and thus affect the actual composite effect.

[0082] Comparative Example 7

[0083] Compared with Example 1, the difference is that in step (3), the composite solvent is changed from deionized water to half ethanol and half deionized water, and the other conditions are consistent with Example 1. The CO yield rate is 14.19 μmol / (g·h).

[0084] Comparative Example 8

[0085] Compared with Example 1, the difference is that in step (1), the molar ratio of raw materials BaCO3 and SrCO3 during preparation is changed from 1:1 to 3:7, and other conditions are consistent with Example 1. The obtained composite catalyst is named 10% ReS2-Ba 0.3 Sr 0.7 TiO3.

[0086] The 10% ReS2-Ba 0.3 Sr 0.7 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 5.18 μmol / (g·h).

[0087] Comparative Example 9

[0088] Compared with Example 1, the difference is that in step (1), the molar ratio of raw materials BaCO3 and SrCO3 during preparation is changed from 1:1 to 7:3, and other conditions are consistent with Example 1. The obtained composite catalyst is named 10% ReS2-Ba 0.7 Sr 0.3 TiO3.

[0089] The 10% ReS2-Ba 0.7 Sr 0.3 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 17.09 μmol / (g·h).

[0090] Comparative Example 10

[0091] The catalyst of Comparative Example 10 is pure BaTiO3. The preparation method is the same as step (1) of Example 1, except that SrCO3 is not added to the raw materials during the preparation.

[0092] The BaTiO3 of Comparative Example 10 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those of Example 1, and the CO yield was 1.72 μmol / (g·h).

[0093] Comparative Example 11

[0094] The catalyst of Comparative Example 10 is pure SrTiO3. The preparation method is the same as step (1) of Example 1, except that BaCO3 is not added to the raw materials during the preparation.

[0095] The pure SrTiO3 catalyst of Comparative Example 11 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those of Example 1, and the CO yield was 2.03 μmol / (g·h).

[0096] Comparative Example 12

[0097] Compared with Example 1, the difference is that in step (3), the co-catalyst added during the compounding is changed from ReS2 to Co9S8, and the obtained composite catalyst is named 10% Co9S8-Ba 0.5 Sr 0.5 TiO3.

[0098] The 10% Co9S8-Ba 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 15.14 μmol / (g·h).

[0099] Comparative Example 13

[0100] Compared with Example 1, the difference is that in step (3), the co-catalyst added during the compounding is changed from ReS2 to Cu7S4, and the obtained composite catalyst is named 10% Cu7S4-Ba 0.5 Sr 0.5 TiO3.

[0101] The 10% Cu7S4-Ba 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were consistent with those in Example 1, and the CO yield was 5.24 μmol / (g·h).

[0102] Comparative Example 14

[0103] Compared with Example 1, the difference is that in step (1), the temperature of solid phase calcination is changed from 800°C to 700°C, and the other conditions are the same as those in Example 1. The obtained composite catalyst is named 700-10% ReS2-Ba 0.5 Sr 0.5 TiO3.

[0104] The 700-10% ReS2-Ba 0.5 Sr 0.5 TiO3 was used for piezoelectric catalytic reduction of carbon dioxide. The experimental conditions were the same as those in Example 1, and the CO yield was 1.65 μmol / (g·h). This is because calcination at 700°C cannot accurately produce Ba 0.5 Sr 0.5 TiO3. The characteristic peaks on XRD cannot accurately correspond to the PDF card, and there are a lot of impurity peaks, indicating that Ba cannot be completely formed at 700℃. 0.5 Sr 0.5 TiO3, there are a lot of intermediate impurities, the specific XRD diagram is shown in Fig.11 .

[0105] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A ReS2 / Ba 0.5 Sr 0.5 The TiO3 composite catalyst is characterized in that ReS2 and Ba 0.5 Sr 0.5 After mixing with TiO3, ReS2 / Ba was formed by solvent evaporation method. 0.5 Sr 0.5 TiO3 composite; the ReS2 is Ba 0.5 Sr 0.5 5-15% of the mass of TiO3.

2. A ReS2 / Ba according to claim 1 0.5 Sr 0.5 The method for preparing a TiO3 composite catalyst is characterized in that: ReS2 and Ba 0.5 Sr 0.5 TiO3 was added to deionized water, and then subjected to ultrasonic and stirring composite treatment, and then filtered, washed, and dried to finally obtain ReS2 / Ba 0.5 Sr 0.5 TiO3 composite catalyst.

3. ReS2 / Ba according to claim 2 0.5 Sr 0.5 The method for preparing a TiO3 composite catalyst is characterized in that: ReS2 is Ba 0.5 Sr 0.5 7.5-10% of the mass of TiO3.

4. ReS2 / Ba according to claim 2 0.5 Sr 0.5 The method for preparing a TiO3 composite catalyst is characterized in that: Ba 0.5 Sr 0.5 The preparation method of TiO3 is as follows: tetrabutyl titanate is added to anhydrous ethanol, BaCO3 and SrCO3 are added after sufficient stirring, and solution A is obtained by ultrasonic treatment. Deionized water, HCl and anhydrous ethanol are mixed and stirred to obtain solution B. Solution B is then added dropwise into solution A to obtain a mixed solution in a gel state, which is then vacuum dried overnight to obtain a xerogel barium strontium titanate precursor. A certain amount of the precursor is placed in a tube furnace and fully calcined to obtain a white product Ba 0.5 Sr 0.5 The molar ratio of TiO3, BaCO3 and SrCO3 is 1:1, the calcination temperature in the tubular furnace is 800-900°C, and the calcination time is 6-10h.

5. A ReS2 / Ba as claimed in claim 1 0.5 Sr 0.5 The application of TiO3 composite catalyst in piezoelectric photocatalytic reduction of carbon dioxide is characterized in that: ReS2 / Ba 0.5 Sr 0.5 The TiO3 composite catalyst is added to water and dispersed evenly, and then CO2 is introduced to carry out piezoelectric photocatalytic reduction of carbon dioxide under the synergistic effect of ultrasound and light.

6. The use according to claim 5, characterized in that: The ultrasonic power is 200-300W; the light source is sunlight.

7. The use according to claim 5, characterized in that: The ReS2 / Ba 0.5 Sr 0.5 The dosage of TiO3 composite catalyst in water is 1-5 mg / 20 mL.

Citation Information

Patent Citations

  • Integrated assembly and method of forming integrated assembly

    CN114121957A

  • Semiconductor laser element with Fermi surface topological layer

    CN116646822A

  • Process for the manufacture of carbamates

    US4258201A