Preparation method and application of nitrogen-doped graphene catalyst taking CO2 as carbon source

The conversion of CO2 into nitrogen-doped graphene catalyst through coupling reaction method has solved the problem of high equipment and low conversion in the prior art, and achieved high atomic economic and high activity graphene preparation, which is suitable for fuel cells Production.

CN118925778APending Publication Date: 2024-11-12WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068610.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the method of converting CO2 into graphene has problems such as high equipment demand, low conversion rate, high cost and many by-products, making it difficult to achieve high atomic economy and large-scale production.

Method used

Coupling reaction method is used to react CO2 with propargyl alcohol and pyrrolidine to form a copper nitrogen carbon precursor, and coupled with copper phthalocyanine on a halogen salt template to prepare a nitrogen-doped graphene catalyst, reducing equipment demand and increasing atoms Economy and productivity.

Benefits of technology

It has achieved low equipment demand, high atomic economy, and no by-product preparation of nitrogen-doped graphene catalysts, with high oxygen reduction reaction activity and stability, suitable for fuel cells, and is easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004980127630000011
    Figure HDA0004980127630000011
  • Figure HDA0004980127630000012
    Figure HDA0004980127630000012
  • Figure HDA0004980127630000013
    Figure HDA0004980127630000013
Patent Text Reader

Abstract

The invention discloses a preparation method of a nitrogen-doped graphene catalyst taking CO2 as a carbon source. The preparation method comprises the following steps: S1, preparing hydrogel; s2, reacting propargyl alcohol, pyrrolidine and CO2 to obtain a copper-nitrogen-carbon precursor; s3, grinding the copper-nitrogen-carbon precursor, copper phthalocyanine and haloid; and S4, sequentially calcining, cooling, washing and drying in a tubular furnace, so that the copper-nitrogen-carbon precursor and copper phthalocyanine are coupled on the haloid template to obtain the nitrogen-doped graphene catalyst. The nitrogen-doped graphene catalyst has high specific surface area and rich nitrogen active sites, and can be used for oxygen reduction reaction. According to the method, the greenhouse gas CO2 is converted into high-addition nitrogen-doped graphene by adopting a coupling reaction way, waste is turned into wealth, the atom economy is high, the operation is simple, and large-scale production is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanomaterials and relates to a preparation method and application of a nitrogen-doped graphene catalyst using CO2 as a carbon source. Background Art

[0002] Currently, the conversion of CO2 into small organic molecules such as urea, methanol, carbonates, ethylene, glucose, fatty acids and hydrocarbons has been widely studied. However, the number of products produced using these methods is small, and the reactions require high energy and precise control, which limits the commercial benefits of CO2 capture and utilization.

[0003] Graphene is a complex sp 2 The new generation of polymer materials with bonded carbon structures have good electrical, optical, thermal and mechanical properties, and have broad application prospects in the fields of sensors, electrodes, electronics and energy storage. However, the preparation of graphene and its functionalization using CO2 are highly challenging. Although some methods have been developed to synthesize graphene or graphene-like materials using CO2 as a carbon source, including chemical vapor deposition (CVD) and molten salt electrolysis, these methods require expensive equipment, have low conversion rates and high costs due to the stability of the carbon-oxygen double bonds in CO2. So far, no method has been found to easily synthesize graphene or graphene-like materials with high atom economy using CO2. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a nitrogen-doped graphene catalyst using CO2 as a carbon source in view of the deficiencies in the above-mentioned prior art. The coupling reaction pathway of the present invention uses CO2 as a carbon source to convert graphene. Compared with the existing CO2 preparation technology for graphene, such as molten salt electroreduction of CO2, CVD and other methods, the equipment requirements are low, the atom economy is good, and there are no other by-products. The prepared nitrogen-doped graphene catalyst has high ORR catalytic activity and stability.

[0005] The technical solution adopted by the present invention to solve the above-mentioned problems is:

[0006] A method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source comprises the following steps:

[0007] S1, adding the catalyst copper salt to a mixture reactor of propargyl alcohol and pyrrolidine, stirring at room temperature to make the catalyst copper salt evenly dispersed in the mixed solution to prepare a hydrogel;

[0008] S2, introducing CO2 into the reactor described in step S1, maintaining a temperature of 45°C to 60°C for reaction for 12 to 24 hours to obtain a copper nitrogen carbon precursor;

[0009] S3, mixing copper phthalocyanine with the copper nitrogen carbon precursor obtained in step S2, and adding a halogen salt as a template and a dispersant for grinding to obtain a uniformly dispersed blue powder mixture;

[0010] S4, calcining the blue powder mixture described in step S3, and then cooling, washing, and drying, so that the copper nitrogen carbon precursor and copper phthalocyanine are coupled on the halogen salt template to obtain a nitrogen-doped graphene catalyst.

[0011] According to the above scheme, in step S1, the propargyl alcohol is one or a mixture of any proportion of 2-methyl-3-butyn-2-ol, 2-ethyl-3-butyn-2-ol, 2-propyl-3-butyn-2-ol, 2-phenyl-3-butyn-2-ol, etc.

[0012] According to the above scheme, in step S1, the molar ratio of copper salt to propargyl alcohol is 0.05:1 to 0.3:1 (preferably 0.1:1 to 0.2:1), and the molar ratio of propargyl alcohol to pyrrolidine is 1:0.5 to 1:2.

[0013] According to the above scheme, in step S1, the catalyst copper salt is evenly dispersed in the mixed solution under stirring at room temperature for 3 to 4 hours to obtain a hydrogel state without obvious copper salt precipitation.

[0014] According to the above scheme, in step S1, the copper salt is one or a mixture of several of copper chloride, copper iodide, copper bromide, etc. in any proportion.

[0015] According to the above scheme, in step S2, CO2 is introduced into the reactor, and the amount introduced is preferably maintained at a pressure of 1 to 2 bar.

[0016] According to the above scheme, in step S3, the halogen salt is selected from one or more of potassium chloride, potassium carbonate, sodium chloride, etc.; the mass ratio of copper phthalocyanine to copper nitrogen carbon precursor is 5-20:1, and the mass ratio of copper phthalocyanine to halogen salt is 1:50-200.

[0017] According to the above scheme, in step S3, a ball mill is used for grinding, the ball milling time is 1 to 3 hours, the given frequency is about 24 Hz, and the ball milling interval is about 5 minutes.

[0018] According to the above scheme, in step S4, nitrogen or inert gas is used as the protective atmosphere for calcination, the carbonization temperature is 600°C to 800°C, the heating rate is 5°C / min, and the carbonization time is 9 to 12h.

[0019] The nitrogen-doped graphene catalyst prepared by the above method can be used in oxygen reduction reaction (ORR).

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention first obtains a copper nitrogen carbon precursor by reacting propargyl alcohol, pyrrolidine and CO2, and uses copper phthalocyanine as a precursor to couple with the copper nitrogen carbon precursor on a halogen salt template to prepare nitrogen-doped graphene. The present invention uses an organic synthesis method to convert graphene using CO2 as a carbon source, which is an innovative method. Compared with existing CO2 graphene preparation technologies such as molten salt electroreduction of CO2, CVD and other methods, the equipment requirements are low, the atom economy is good, and there are no other by-products.

[0022] 2. The nitrogen-doped graphene catalyst prepared by the present invention uses nitrogen-containing pyrrolidine and copper phthalocyanine as raw materials for nitrogen doping during the synthesis process, so there is no need for an additional nitrogen doping step, and the prepared graphene has abundant nitrogen-doped active sites.

[0023] 3. The nitrogen-doped graphene catalyst prepared by the present invention has a thin two-dimensional sheet structure and a large specific surface area because it adopts the salt template method.

[0024] 3. The present invention does not require expensive equipment, and the catalyst has a high yield and high atom economic benefit, and can be synthesized in large quantities for industrial large-scale production.

[0025] 4. The nitrogen-doped graphene catalyst prepared by the present invention has high ORR catalytic activity and stability and can be used as a fuel cell with excellent performance.

[0026] The present invention adopts a coupling reaction approach to convert greenhouse gas CO2 into a high-added nitrogen-doped graphene electrocatalyst, turning waste into treasure, with high atomic economy, simple operation, and easy large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a scanning electron microscope image of the nitrogen-doped graphene catalyst prepared in Example 1;

[0028] Figure 2 This is a transmission electron microscopy image of the nitrogen-doped graphene catalyst prepared in Example 1;

[0029] Figure 3 The X-ray diffraction pattern of the nitrogen-doped graphene catalyst prepared in Example 1;

[0030] Figure 4 N2 adsorption-desorption curve of the nitrogen-doped graphene catalyst prepared in Example 1;

[0031] Figure 5 X-ray photoelectron spectrum of the nitrogen-doped graphene catalyst prepared in Example 1;

[0032] Figure 6 This is a scanning electron microscope image of the nitrogen-doped graphene catalyst prepared in Example 2;

[0033] Figure 7ORR polarization curves of the nitrogen-doped graphene catalyst prepared in Example 1 and the commercial Pt / C (20%) catalyst in 0.1M KOH solution, respectively;

[0034] Figure 8 The stability test of the nitrogen-doped graphene catalyst prepared in Example 1 in 0.1M KOH solution;

[0035] Fig. 9 X-ray photoelectron spectrum of the catalyst prepared in Comparative Example 3;

[0036] Fig.10 ORR polarization curve of commercial Pt / C (20%) catalyst of nitrogen-doped graphene catalyst prepared in Comparative Example 3 in 0.1 M KOH solution;

[0037] Fig.11 This is a scanning electron microscope image of the sample prepared in Comparative Example 4.

[0038] Fig.12 This is a scanning electron microscope image of the sample prepared in Comparative Example 5. DETAILED DESCRIPTION

[0039] The following examples further illustrate the contents of the present invention so that those skilled in the art can better understand the present invention and implement it, and should not be construed as limiting the scope of protection of the present invention.

[0040] Example 1

[0041] A method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source, the specific steps are as follows:

[0042] S1, adding 0.134g of cupric chloride into a reactor containing 1.46g of 2-phenyl-3-butyn-2-ol and 0.71g of pyrrolidine (the molar ratio of cupric chloride, 2-phenyl-3-butyn-2-ol and pyrrolidine is 0.1:1:1), stirring at room temperature to uniformly disperse the catalyst copper salt in the mixed solution to obtain a hydrogel;

[0043] S2, introducing CO2 into the reactor in step S1, maintaining the introduction amount of CO2 at 1-2 bar, maintaining the temperature at 45° C. for 12 hours to obtain a copper nitrogen carbon precursor;

[0044] S3, adding 20 g of copper phthalocyanine to a ball mill containing the copper nitrogen carbon precursor (2 g) obtained in step S2, and adding 2000 g of potassium chloride as a template and dispersant, the ball milling time is 2 hours, the given frequency is 24 Hz, the ball milling interval is 5 minutes, and drying is performed to obtain a blue powder mixture;

[0045] S4. The blue powder mixture obtained in step S3 is charged into a tubular furnace for calcination to achieve carbonization. The protective gas is nitrogen. The carbonization temperature is 600° C., the heating rate is 5° C. / min, and the carbonization time is 9 hours. The mixture is then cooled, washed, and dried to obtain graphene-based carbon nanosheets, i.e., nitrogen-doped graphene catalysts.

[0046] The graphene-based carbon nanosheets prepared in this example were tested by scanning electron microscopy, and the SEM morphology was obtained. Figure 1 , showing the extremely thin lamellar structure of the sample.

[0047] The graphene-based carbon nanosheets prepared in this example were tested by transmission electron microscopy, and the TEM images were obtained. Figure 2 , further showing the graphene sheet structure of the sample.

[0048] The XRD pattern of the graphene-based carbon nanosheets prepared in this example is shown in Figure 3 , the sample has characteristic diffraction peaks of graphite and characteristic diffraction peaks of Cu.

[0049] The graphene-based carbon nanosheets prepared in this embodiment were subjected to N2 adsorption and desorption tests, and the N2 adsorption and desorption results were obtained. Figure 4 , showing the high specific surface area of ​​the sample.

[0050] The graphene-based carbon nanosheets prepared in this example were tested by X-ray photoelectron spectroscopy, and the X-ray photoelectron spectroscopy test was performed. Figure 5 , showing the sample’s abundant nitrogen active sites.

[0051] The graphene-based carbon nanosheets prepared in Example 1 were tested for their ORR catalytic performance and stability. The specific process was as follows: Preparation of glassy carbon rotating disk electrode: 2 mg of graphene-based carbon nanosheet powder prepared in Example 1 was dispersed in 950 μL of ethanol and 50 μL of 5% Nafion solution to form a uniform suspension (2 mg mL -1 ) to prepare the working electrode, and deposit 15 μL of the suspension on a 5 mm diameter (0.196 cm area) 2 ) on the surface of a glassy carbon rotating disk electrode; then the electrochemical test was performed on an Autolab PGSTAT 30 workstation, using Ag / AgCl as the reference electrode and a carbon rod as the reference electrode, using a three-electrode system for electrochemical measurements. First, at a rotation speed of 1600 rpm and a scan rate of 10 mVs -1 The ORR polarization curve was tested in 0.1M KOH solution, see Figure 7 , which has a similar half-step potential and starting voltage to the commercial platinum-carbon catalyst, indicating that it has efficient electrocatalytic performance; then at a scan rate of 50 mVs -1The cycle stability and it curve were tested in 0.1M KOH solution. Figure 8 , which is much higher than the stability of commercial platinum-carbon catalysts, indicating that it has high stability.

[0052] Example 2

[0053] A method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source, the specific steps are as follows:

[0054] S1, adding 0.268 g of cupric chloride into a reactor containing 2.92 g of 2-phenyl-3-butyn-2-ol and 1.42 g of pyrrolidine, stirring at room temperature to uniformly disperse the catalyst copper salt in the mixed solution, to prepare a hydrogel;

[0055] S2, introducing CO2 into the reactor described in step S1, maintaining the temperature at 45°C for 12 hours, and maintaining the introduction amount of CO2 at 1 bar to obtain a copper nitrogen carbon precursor;

[0056] S3, adding 40g of copper phthalocyanine and 4000g of potassium chloride into a ball mill containing 4g of copper nitrogen carbon precursor obtained in step S2, the ball milling time is 2 hours, the given frequency is 24 Hz, the ball milling interval is 5 minutes, and drying is performed to obtain a blue powder mixture;

[0057] S4. The blue powder mixture obtained in step S3 is placed in a tubular furnace for calcination. The protective gas is nitrogen. The carbonization temperature is 600°C, the heating rate is 5°C / min, and the carbonization time is 9h. The sample is then cooled, washed, and dried in sequence.

[0058] The graphene-based carbon nanosheets prepared in this example were tested by scanning electron microscopy, and the SEM morphology was obtained. Figure 6 , and also shows the extremely thin layer structure of the sample. Step S1 expands the reactants compared with Example 1, and the sample changes are not obvious.

[0059] Example 3

[0060] This embodiment is substantially the same as embodiment 1, except that: S1, 0.317 g of copper iodide is added to 1.46 g of 2-phenyl-3-butyn-2-ol and 0.71 g of pyrrolidine (i.e., the molar ratio of copper chloride, 2-phenyl-3-butyn-2-ol, and pyrrolidine is 0.2:1:1).

[0061] Example 4

[0062] This embodiment is substantially the same as embodiment 1, except that: S3, 20 g of copper phthalocyanine and 1000 g of potassium chloride are added to a ball mill containing the copper nitrogen carbon precursor in step S2, and ground and dried to obtain a blue powder mixture.

[0063] Example 5

[0064] This embodiment is substantially the same as embodiment 1, except that: S4, the blue powder mixture obtained in step S3 is charged into a tubular furnace for calcination to achieve carbonization, the carbonization temperature is 800°C, the heating rate is 5°C / min, the carbonization time is 9h, and then cooled, washed, and dried in sequence to obtain graphene-based carbon nanosheets.

[0065] Comparative Example 1

[0066] The difference between this comparative example and Example 1 is that: S2, no CO2 is introduced into the reactor, and the copper nitrogen carbon precursor cannot be obtained. Because without the introduction of CO2, propargyl alcohol and pyrrolidine cannot undergo an organic reaction to generate β-carbonyl carbamate, and cannot couple with copper phthalocyanine.

[0067] Comparative Example 2

[0068] The difference between this comparative example and Example 1 is that: S1, no pyrrolidine is added; S2, CO2 is introduced into the reactor described in step S1, the temperature is maintained at 45°C for 12 hours, and the amount of CO2 introduced is maintained at 1 bar. A copper nitrogen-carbon precursor cannot be obtained because propargyl alcohol and CO2 form cyclic carbonate compounds, which are unstable and easily decomposed, and cannot be coupled with copper phthalocyanine.

[0069] Comparative Example 3

[0070] The difference between this comparative example and Example 1 is that:

[0071] S3, adding copper-free nitrogen-carbon precursor, grinding 3 g of copper phthalocyanine and 150 g of potassium chloride in a ball mill, and drying to obtain a blue powder mixture;

[0072] S4. The blue powder mixture obtained in step S3 is placed in a tubular furnace for calcination. The protective gas is nitrogen. The carbonization temperature is 600° C., the heating rate is 5° C. / min, and the carbonization time is 9 hours. The mixture is then cooled, washed, and dried in sequence to obtain a sample.

[0073] The samples prepared in Comparative Example 3 were tested for X-ray photoelectron spectroscopy, and the results are shown in Fig. 9 , the N doping content is significantly lower than that in Example 1; at the same time, its ORR performance is tested, and the results are shown in Fig.10 , and its catalytic performance is also significantly reduced, indicating that the addition of copper nitrogen carbon precursor can increase its nitrogen doping content and thus improve its electrocatalytic performance.

[0074] Comparative Example 4

[0075] The difference between this comparative example and Example 1 is that:

[0076] S3, without the addition of copper phthalocyanine, the copper nitrogen carbon precursor (2 g) was added into a ball mill, and 1000 g of potassium chloride was added as a template and dispersant, and the mixture was ground and dried to obtain a white powder mixture;

[0077] S4. The white powder mixture obtained in step S3 is placed in a tubular furnace for calcination. The protective gas is nitrogen. The carbonization temperature is 600° C., the heating rate is 5° C. / min, and the carbonization time is 9 hours. The mixture is then cooled, washed, and dried in sequence to obtain a sample.

[0078] The graphene-based carbon nanosheets prepared in this comparative example were subjected to electron microscope scanning to obtain a SEM morphology. Fig.11 , no graphene sheet structure; at the same time, its ORR performance was tested and there was no catalytic activity, indicating that the formation of graphene structure requires the participation of copper phthalocyanine.

[0079] Comparative Example 5

[0080] The difference between this comparative example and Example 1 is that:

[0081] S3, without the addition of halogen salt, add copper nitrogen carbon precursor (2 g) and 1.5 g copper phthalocyanine into a ball mill, grind and dry to obtain a blue powder mixture;

[0082] S4. The blue powder mixture obtained in step S3 is placed in a tubular furnace for calcination. The protective gas is nitrogen. The carbonization temperature is 600° C., the heating rate is 5° C. / min, and the carbonization time is 9 hours. The mixture is then cooled, washed, and dried in sequence to obtain a sample.

[0083] The graphene-based carbon nanosheets prepared in this comparative example were subjected to electron microscope scanning to obtain a SEM morphology. Fig.12 , there is no graphene sheet structure, indicating that the formation of graphene structure requires the participation of template agent.

[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source, characterized in that: The following steps are involved: S1, adding the catalyst copper salt to a mixture reactor of propargyl alcohol and pyrrolidine, stirring at room temperature to make the catalyst copper salt evenly dispersed in the mixed solution to prepare a hydrogel; S2, introducing CO2 into the reactor described in step S1, maintaining a temperature of 45°C to 60°C for reaction for 12 to 24 hours to obtain a copper nitrogen carbon precursor; S3, mixing copper phthalocyanine with the copper nitrogen carbon precursor obtained in step S2, and adding a halogen salt as a template and a dispersant for grinding to obtain a uniformly dispersed blue powder mixture; S4, calcining the blue powder mixture in step S3, and then cooling, washing and drying to obtain a nitrogen-doped graphene catalyst.

2. The method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S1, the propargyl alcohol is one of 2-methyl-3-butyn-2-ol, 2-ethyl-3-butyn-2-ol, 2-propyl-3-butyn-2-ol, 2-phenyl-3-butyn-2-ol, or a mixture of any proportions thereof.

3. The method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S1, the molar ratio of copper salt to propargyl alcohol is 0.05:1 to 0.3:1, and the molar ratio of propargyl alcohol to pyrrolidine is 1:0.5 to 1:

2.

4. The method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S1, the catalyst copper salt is evenly dispersed in the mixed solution under stirring at room temperature for 3 to 4 hours to obtain a hydrogel without obvious copper salt precipitation.

5. The method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S1, the copper salt is one of copper chloride, copper iodide, and copper bromide, or a mixture of several of them in any proportion.

6. The method for preparing a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S2, the amount of CO2 introduced is maintained at a pressure of 1 to 2 bar.

7. The preparation method and application of a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S3, the halogen salt is selected from one or more of potassium chloride, potassium carbonate, and sodium chloride; the mass ratio of copper phthalocyanine to copper nitrogen carbon precursor is 5-20:1, and the mass ratio of copper phthalocyanine to halogen salt is 1:50-200.

8. The preparation method and application of a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: The grinding is carried out using a ball mill, the ball milling time is 1 to 3 hours, the given frequency is 20 to 30 Hz, and the ball milling interval is 4 to 6 minutes.

9. The preparation method and application of a nitrogen-doped graphene catalyst using CO2 as a carbon source according to claim 1, characterized in that: In step S4, nitrogen or inert gas is used as a protective atmosphere for calcination, the calcination temperature is 600° C. to 800° C., and the calcination time is 9 to 12 hours.

10. Use of the nitrogen-doped graphene catalyst prepared by the method of any one of claims 1 to 9 in redox reactions.