Rhodium-based catalyst as well as preparation method and application thereof

By preparing the rhodium-based catalyst of TiOx-SiO2 support, the problems of difficulty in recovering catalysts and low activity of water-oil heterogeneous catalytic system in the hydroformylation reaction are solved, and high activity and stability are achieved, and the potential of industrial catalysts are achieved.

CN118925796APending Publication Date: 2024-11-12SHANDONG CHAMBROAD PETROCHEMICALS CO LTD

Patent Information

Application Number
CN202410972544.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing hydroformylation catalysts are difficult to recover in the reaction, and the water-oil heterogeneous catalytic system has low activity, resulting in high production costs and poor catalyst stability.

Method used

The rhodium-based catalyst using TiOx-SiO2 as the support is prepared by impregnation and calcination, and the loading amount and particle size of the rhodium are controlled to form a highly active and easy-to-separate catalyst.

Benefits of technology

It realizes high activity and easy recycling of the catalyst, reduces production costs, and improves the stability of the catalyst, and has the potential for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004953647020000011
    Figure HDA0004953647020000011
  • Figure HDA0004953647020000012
    Figure HDA0004953647020000012
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to a rhodium-based catalyst and a preparation method and application thereof. The rhodium-based catalyst comprises a carrier and an active component, the carrier is TiOx-SiO2, and the active component is rhodium; in the rhodium-based catalyst, the loading amount of rhodium is 0.03-0.2% of the total weight of the catalyst. The immobilized rhodium-based catalyst is prepared, the particle size of the immobilized rhodium-based catalyst is controlled, so that the advantage of heterogeneous catalysis and easy separation of the immobilized rhodium-based catalyst is exerted, meanwhile, the catalytic activity is improved, and the preparation is simple and easy to industrialize. The rhodium-based catalyst has high activity, is easy to separate and recover from reactants, solves the problems of complex separation process of a homogeneous catalyst and a product and difficult recovery of noble metals, overcomes the problem of low activity of a water-oil heterogeneous catalytic system, and has the potential of becoming an industrial catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a rhodium-based catalyst, a preparation method and application thereof. Background Art

[0002] The hydroformylation reaction is a process of synthesizing aldehydes using olefins and synthesis gas (CO and H2) as raw materials in the presence of a catalyst. Further reduction, oxidation, etherification, esterification, condensation and other reactions can produce a series of alcohols, ethers, amines, acids, esters, aldehydes and acids. It is widely used in the preparation of chemical products such as fragrances, gasoline additives, resins and surfactants, and has become one of the most important chemical reactions in today's industrial applications.

[0003] At present, most of the mainstream hydroformylation catalysts are third-generation oil-soluble carbonyl rhodium phosphine catalysts and fourth-generation water-soluble rhodium phosphine catalysts, which can be carried out under mild conditions of low temperature and low pressure, but the problem of difficulty in recovering the rhodium catalyst during the hydroformylation reaction is prone to occur, which greatly increases the production cost. The water-soluble rhodium phosphine catalyst uses an oil-water two-phase reaction system to effectively separate the product from the catalyst, which to a certain extent solves the problem of catalyst recovery in the olefin hydroformylation process, but the catalyst has high energy consumption in the oil-water two-phase separation, and its catalytic activity needs to be further improved.

[0004] Therefore, researchers have turned their attention to solid-oil heterogeneous catalytic systems, but most of the catalytic effects, regional selectivity and stability need to be improved. For example, the 0.006% rhodium / ZnO catalyst reported by Zhang Tao's research group at the Dalian Institute of Chemical Physics has higher catalytic activity than traditional carbonyl rhodium catalysts, but the catalyst stability is poor (Angew. Chem. Int. Ed., 2016; 55: 16054-16058). Huang Wenyu's research group at Iowa State University reported the preparation of SBA-15 stabilized rhodium Zn alloy as rhodium Zn / SBA-15, and its catalytic activity and stability were improved (J. Am. Chem. Soc., 2021; 49: 20907–20915). Although the above catalysts have played the advantages of heterogeneous catalysts in solid-oil heterogeneous catalytic systems, they are difficult to prepare and the cost needs to be further controlled. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a rhodium-based catalyst, a preparation method and application thereof. The rhodium-based catalyst provided by the present invention has high activity and is easy to separate and recover from reactants, solving the problems of complex separation process between homogeneous catalysts and products and difficulty in recovering precious metals. At the same time, it overcomes the low activity problem of water-oil heterogeneous catalytic systems and has the potential to become an industrial catalyst.

[0006] The present invention provides a rhodium-based catalyst, comprising: a carrier and an active component;

[0007] The carrier is TiOx-SiO2, and the active component is rhodium;

[0008] In the rhodium-based catalyst, the loading amount of rhodium is 0.03% to 0.2% of the total weight of the catalyst.

[0009] Preferably, in the rhodium-based catalyst, the mass content of Ti is 0.3% to 0.5%, and the molar ratio of silicon to titanium is (25 to 45):1.

[0010] Preferably, the pore size of the rhodium-based catalyst is 80 to 200 nm, and the specific surface area is 260 to 400 m 2 / g, pore volume is 0.3~0.5mL / g, and particle size is 10~80 mesh.

[0011] The present invention also provides a method for preparing the above-mentioned rhodium-based catalyst, comprising the following steps:

[0012] S1) dispersing rhodium salt in saturated ammonia water, adjusting the pH value to 7 to 10, and obtaining an impregnation solution;

[0013] S2) mixing the impregnation solution with titanium silicon molecular sieve TS-1 for impregnation to obtain an impregnation mixture;

[0014] S3) filtering, drying, and calcining the impregnated mixture to obtain a dry molecular sieve;

[0015] S4) mixing the dry molecular sieve, sesbania powder, silica sol and liquid paraffin, and shaping them to obtain a rhodium-based catalyst.

[0016] Preferably, in step S1), the rhodium salt comprises one or two of rhodium chloride, ammonium chlororhodate and chlororhodic acid;

[0017] The rhodium salt is dispersed in a rhodium salt solution formed by ammonia water, and the concentration of rhodium is 0.002-0.4 mol / L.

[0018] Preferably, in step S2), the mass ratio of the impregnation solution to the titanium silicon molecular sieve TS-1 is (50-100):1;

[0019] The immersion time is 0.5 to 4 hours.

[0020] Preferably, in step S3), after the drying, the step further comprises: heating to a calcination temperature; the heating rate is 5 to 10°C / min;

[0021] The calcination temperature is 400-600° C. and the calcination time is 4-8 hours.

[0022] Preferably, in step S4), the solid content of the silica sol is 28% to 35%;

[0023] The mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:1-3:10-40:5-10.

[0024] The present invention also provides a use of the above-mentioned rhodium-based catalyst or the rhodium-based catalyst prepared by the above-mentioned preparation method as an isopentene hydroformylation catalyst.

[0025] Preferably, the reaction raw materials for isopentene hydroformylation include CO, H2 and isopentene; the reaction raw materials undergo isopentene hydroformylation reaction under the action of a rhodium-based catalyst;

[0026] The molar ratio of CO to H2 is 0.1 to 2:1;

[0027] The mass ratio of isopentene to the rhodium-containing catalyst is 200-450:0.5-4;

[0028] The temperature of the hydroformylation reaction is 80-130° C., the time is 2-12 hours, and the pressure is 0.5-10 MPa.

[0029] The present invention provides a rhodium-based catalyst, comprising: a carrier and an active component; the carrier is TiOx-SiO2, and the active component is rhodium; in the rhodium-based catalyst, the loading amount of rhodium is 0.03% to 0.2% of the total weight of the catalyst. The present invention prepares a solid-supported rhodium-based catalyst and controls its particle size, thereby giving full play to the advantages of its heterogeneous catalysis and easy separation, while improving the catalytic activity, and the preparation is simple and easy to industrialize. The rhodium-based catalyst has high activity and is easy to separate and recover from reactants, solving the problems of complex separation process of homogeneous catalysts and products and difficulty in recovering precious metals, while overcoming the low activity problem of water-oil heterogeneous catalytic systems, and has the potential to become an industrial catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The gas chromatogram of the reaction product prepared in Example 1 of the present invention;

[0031] Figure 2 This is a gas chromatogram of the reaction product prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The present invention provides a rhodium-based catalyst, comprising: a carrier and an active component;

[0034] The carrier is TiOx-SiO2, and the active component is rhodium;

[0035] In the rhodium-based catalyst, the loading amount of rhodium is 0.03% to 0.2% of the total weight of the catalyst.

[0036] In certain embodiments of the present invention, in the rhodium-based catalyst, the mass content of Ti is 0.3% to 0.5%, preferably 0.35% to 0.45%; the molar ratio of silicon to titanium is (25 to 45):1, preferably (30 to 40):1, such as 30:1.

[0037] In certain embodiments of the present invention, the pore size of the rhodium-based catalyst is 80 to 200 nm, preferably 80 to 150 nm; the specific surface area is 260 to 400 m 2 / g, preferably 300-350m 2 / g; the pore volume is 0.3-0.5 mL / g, preferably 0.35-0.45 mL / g; the particle size is 10-80 mesh, preferably 20-60 mesh.

[0038] In certain embodiments of the present invention, the loading amount of rhodium in the rhodium-based catalyst is 0.1% of the total weight of the catalyst.

[0039] The present invention also provides a method for preparing the rhodium-based catalyst described above, comprising the following steps:

[0040] S1) dispersing rhodium salt in saturated ammonia water, adjusting the pH value to 7 to 10, and obtaining an impregnation solution;

[0041] S2) mixing the impregnation solution with titanium silicon molecular sieve TS-1 for impregnation to obtain an impregnation mixture;

[0042] S3) filtering, drying, and calcining the impregnated mixture to obtain a dry molecular sieve;

[0043] S4) mixing the dry molecular sieve, sesbania powder, silica sol and liquid paraffin, and shaping them to obtain a rhodium-based catalyst.

[0044] Regarding step S1):

[0045] The rhodium salt is dispersed in saturated ammonia water, and the pH value is adjusted to 7-10 to obtain an impregnation solution.

[0046] In certain embodiments of the present invention, the rhodium salt is selected from one or two of rhodium chloride, ammonium chlororhodate and chlororhodic acid. The rhodium salt is dispersed in saturated ammonia water, and the concentration of rhodium is 0.002-0.4 mol / L, preferably 0.0025-0.35 mol / L, such as 0.1 mol / L.

[0047] Regarding step S2):

[0048] The impregnation solution is mixed with titanium silicon molecular sieve TS-1 for impregnation to obtain an impregnation mixture.

[0049] In certain embodiments of the present invention, the titanium silicon molecular sieve TS-1 is synthesized by a hydrothermal method, which is not particularly limited in the present invention, and specifically comprises the following steps:

[0050] a) mixing a silicon source, a titanium source, a template and an alkali source;

[0051] b) mixing the mixed system obtained in step a) with the nano TS-1 mother solution for crystallization;

[0052] c) solid-liquid separation, washing, drying and calcining the obtained solid to obtain titanium silicon molecular sieve TS-1.

[0053] Step a):

[0054] The silicon source is silica gel with a mass concentration of 25% to 35%; the titanium source is titanium tetrachloride; the template agent is tetrapropylammonium bromide; the alkali source is an ethylamine aqueous solution with a mass concentration of 60% to 70%. The molar ratio of silicon element, titanium tetrachloride, tetrapropylammonium bromide and ethylamine in the silica gel is 0.8 to 1.2: 0.03 to 0.04: 0.1 to 0.2: 0.8 to 1.2; for example, 1: 0.035: 0.15: 1, 1: 0.025: 0.15: 1.

[0055] Step b):

[0056] The nano TS-1 mother solution is used as a crystal seed. The crystallization time is 70 to 74 hours.

[0057] Step c):

[0058] The calcination temperature is 400-600° C., preferably 450-550° C., such as 500° C.; the calcination time is 4-8 hours, preferably 5-7 hours, such as 6 hours.

[0059] In certain embodiments of the present invention, the pore size of the titanium silicalite TS-1 is 80 to 200 nm.

[0060] After obtaining the titanium silicate molecular sieve TS-1, the impregnation solution is mixed with the titanium silicate molecular sieve TS-1 for impregnation.

[0061] The mass ratio of the impregnation solution to the titanium silicon molecular sieve TS-1 is (50-100):1, preferably (60-80):1, such as 70:1.

[0062] The immersion time is 0.5 to 4 hours, preferably 1 to 2 hours.

[0063] Regarding step S3):

[0064] The impregnation mixture is filtered, dried, and then calcined to obtain a dry molecular sieve.

[0065] In certain embodiments of the present invention, the drying temperature is 70-90° C. and the drying time is 8-12 hours.

[0066] After the drying, the method further includes: heating to a calcining temperature. The heating rate is 5 to 10°C / min, such as 10°C / min. The calcining temperature is 400 to 600°C, such as 500°C or 600°C; the calcining time is 4 to 8 hours, specifically 4 hours or 8 hours. After the calcining, the method further includes: naturally cooling to room temperature.

[0067] Regarding step S4):

[0068] The dry molecular sieve, sesbania powder, silica sol and liquid paraffin are mixed and molded to obtain a rhodium-based catalyst.

[0069] In some embodiments of the present invention, the solid content of the silica sol is 28% to 35%, such as 30% to 35%. The mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:1 to 3:10 to 40:5 to 10, preferably 100:2 to 3:25 to 35:7 to 10, such as 100:3:30:10, 100:3:30:8, 100:1.5:15:5.

[0070] The forming is carried out in an extruder, specifically extrusion forming.

[0071] The present invention also provides an application of the above-mentioned rhodium-based catalyst or the rhodium-based catalyst prepared by the above-mentioned preparation method as an isopentene hydroformylation catalyst; specifically, it is applied to a solid-oil two-phase intermittent reactor or fixed bed isopentene hydroformylation reaction.

[0072] The reaction raw materials for isopentene hydroformylation include CO, H2 and isopentene; the reaction raw materials undergo isopentene hydroformylation reaction under the action of a rhodium-based catalyst. The molar ratio of CO to H2 is 0.1 to 2:1, preferably 0.5 to 1.5:1, such as 1:1.

[0073] The mass ratio of isopentene to the rhodium-containing catalyst is 200-450:0.5-4, preferably 250-350:2-3.

[0074] Before the hydroformylation reaction, the method further comprises: heating the temperature to a hydroformylation reaction temperature at a rate of 8 to 12° C. / h, such as 10° C. / h.

[0075] The temperature of the hydroformylation reaction is 80-130° C., preferably 90-120° C., such as 110° C.; the time is 2-12 h, preferably 4-10 h, such as 10 h; the pressure is 0.5-10 MPa, preferably 2-8 MPa, such as 3 MPa.

[0076] After the hydroformylation reaction, the method further comprises: naturally cooling to room temperature and performing vacuum distillation.

[0077] The hydroformylation reaction in the present invention is an atom-economical reaction with high raw material utilization rate. The combination of a rhodium-containing catalyst and an organic phosphine ligand is used. The olefin hydroformylation reaction conditions are mild, and a low-temperature and low-pressure reaction can be achieved. The corresponding aldehyde selectivity is high, the product yield is high, and the use of highly corrosive hydroiodic acid can be avoided.

[0078] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.

[0079] In order to further illustrate the present invention, a rhodium-based catalyst, its preparation method and application provided by the present invention are described in detail below in conjunction with examples, but it should not be understood as limiting the scope of protection of the present invention.

[0080] The raw materials used in the following examples are all commercially available products.

[0081] Example 1

[0082] 1) Preparation of titanium silicate molecular sieve TS-1 by hydrothermal method:

[0083] Silica gel and titanium tetrachloride with a mass concentration of 30% are used as silicon source and titanium source respectively, tetrapropylammonium bromide is used as a template, and an ethylamine aqueous solution with a mass concentration of 65% is used as an alkali source, and the mixture is mixed; the molar ratio of silicon element, titanium tetrachloride, tetrapropylammonium bromide and ethylamine in the silica gel is 1:0.035:0.15:1.

[0084] Nano TS-1 mother liquor was added to the mixed system as a seed crystal, crystallized for 72 hours, solid-liquid separation was performed, the obtained solid was washed and dried, and calcined at 500° C. for 6 hours to obtain titanium silicon molecular sieve TS-1.

[0085] 2) Preparation of rhodium-based catalyst using impregnation drying method:

[0086] 2-1) dispersing rhodium chloride in saturated ammonia water, adjusting the pH value to 7-10, and obtaining a 0.1 mol / L rhodium salt impregnation solution;

[0087] 2-2) adding titanium silicon molecular sieve TS-1 to the impregnation solution, wherein the mass ratio of the impregnation solution to the titanium silicon molecular sieve is 70:1, and impregnating for 72 hours to obtain an impregnation mixture;

[0088] 2-3) filtering the impregnation mixture, drying at 80° C. for 10 h, heating to 500° C. at a rate of 10° C. / min, calcining for 4 h, and naturally cooling to room temperature to obtain a dry molecular sieve;

[0089] 2-4) adding sesbania powder, silica sol and liquid paraffin to the dry molecular sieve, mixing evenly, adding to an extruder for extrusion to obtain a rhodium-based catalyst; the mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:3:30:10.

[0090] The pore size of the rhodium-based catalyst is 120-170 nm, and the specific surface area is 300-400 m 2 , pore volume of 0.3-0.5 mL / g, particle size of 40 mesh; the mass content of Ti is 0.35%, the molar ratio of silicon to titanium is 30:1, and the loading amount of rhodium is 0.1% of the total weight of the catalyst.

[0091] 3) Hydroformylation experiment:

[0092] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0093] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was increased to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0094] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0095] The obtained reaction product is detected by gas chromatography, such as Figure 1 As shown, Figure 1 The gas chromatogram of the reaction product prepared in Example 1 of the present invention. Figure 1 It can be seen that the conversion rate of the raw material isopentene is 93.7% and the selectivity of the target product is 98.3%.

[0096] Example 2

[0097] 1) Preparation of titanium silicate molecular sieve TS-1 by hydrothermal method:

[0098] Silica gel and titanium tetrachloride with a mass concentration of 30% are used as silicon source and titanium source respectively, tetrapropylammonium bromide is used as a template, and an ethylamine aqueous solution with a mass concentration of 65% is used as an alkali source, and the mixture is mixed; the molar ratio of silicon element, titanium tetrachloride, tetrapropylammonium bromide and ethylamine in the silica gel is 1:0.025:0.15:1.

[0099] Nano TS-1 mother liquor was added to the mixed system as a seed crystal, crystallized for 72 hours, solid-liquid separation was performed, the obtained solid was washed and dried, and calcined at 500° C. for 6 hours to obtain titanium silicon molecular sieve TS-1.

[0100] 2) Preparation of rhodium-based catalyst using impregnation drying method:

[0101] 2-1) dispersing rhodium chloride in saturated ammonia water, adjusting the pH value to 7-10, and obtaining a 0.1 mol / L rhodium salt impregnation solution;

[0102] 2-2) adding titanium silicon molecular sieve TS-1 to the impregnation solution, wherein the mass ratio of the impregnation solution to the titanium silicon molecular sieve is 70:1, and impregnating for 72 hours to obtain an impregnation mixture;

[0103] 2-3) filtering the impregnation mixture, drying at 80° C. for 10 h, heating to 500° C. at a rate of 10° C. / min, calcining for 4 h, and naturally cooling to room temperature to obtain a dry molecular sieve;

[0104] 2-4) adding sesbania powder, silica sol and liquid paraffin to the dry molecular sieve, mixing evenly, adding to an extruder for extrusion to obtain a rhodium-based catalyst; the mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:3:30:10.

[0105] The rhodium-based catalyst has a pore size of 140-180 nm and a specific surface area of ​​300-400 m 2 / g, the pore volume is 0.3-0.5mL / g, and the particle size is 40 mesh; the mass content of Ti is 0.3%, the molar ratio of silicon to titanium is 30:1, and the loading amount of rhodium is 0.1% of the total weight of the catalyst.

[0106] 3) Hydroformylation experiment:

[0107] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0108] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was increased to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0109] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0110] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 92.5%, and the selectivity of the target product was 99.3%.

[0111] Example 3

[0112] 1) Preparation of titanium silicate molecular sieve TS-1 by hydrothermal method:

[0113] Same as Example 1.

[0114] 2) Preparation of rhodium-based catalyst using impregnation drying method:

[0115] 2-1) dispersing rhodium chloride in saturated ammonia water, adjusting the pH value to 7-10, and obtaining a 0.1 mol / L rhodium salt impregnation solution;

[0116] 2-2) adding titanium silicon molecular sieve TS-1 to the impregnation solution, wherein the mass ratio of the impregnation solution to the titanium silicon molecular sieve is 70:1, and impregnating for 72 hours to obtain an impregnation mixture;

[0117] 2-3) filtering the impregnation mixture, drying at 80° C. for 10 h, heating to 600° C. at a rate of 10° C. / min, calcining for 4 h, and naturally cooling to room temperature to obtain a dry molecular sieve;

[0118] 2-4) adding sesbania powder, silica sol and liquid paraffin to the dry molecular sieve, mixing evenly, adding to an extruder for extrusion to obtain a rhodium-based catalyst; the mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:3:30:10.

[0119] The pore size of the rhodium-based catalyst is 110-180 nm, and the specific surface area is 300-400 m 2 The pore volume is 0.3-0.5 mL / g and the particle size is 35 mesh; the mass content of Ti is 0.35%, the molar ratio of silicon to titanium is 30:1, and the loading amount of rhodium is 0.1% of the total weight of the catalyst.

[0120] 3) Hydroformylation experiment:

[0121] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0122] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was increased to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0123] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0124] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 93.5%, and the selectivity of the target product was 99.1%.

[0125] Example 4

[0126] 1) Preparation of titanium silicate molecular sieve TS-1 by hydrothermal method:

[0127] Same as Example 1.

[0128] 2) Preparation of rhodium-based catalyst using impregnation drying method:

[0129] 2-1) dispersing rhodium chloride in saturated ammonia water, adjusting the pH value to 7-10, and obtaining a 0.1 mol / L rhodium salt impregnation solution;

[0130] 2-2) adding titanium silicon molecular sieve TS-1 to the impregnation solution, wherein the mass ratio of the impregnation solution to the titanium silicon molecular sieve is 70:1, and impregnating for 72 hours to obtain an impregnation mixture;

[0131] 2-3) filtering the impregnation mixture, drying at 80° C. for 10 h, heating to 500° C. at a rate of 10° C. / min, calcining for 8 h, and naturally cooling to room temperature to obtain a dry molecular sieve;

[0132] 2-4) adding sesbania powder, silica sol and liquid paraffin to the dry molecular sieve and mixing evenly, adding the mixture to an extruder for extrusion to obtain a rhodium-based catalyst; the mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:3:30:8.

[0133] The pore size of the rhodium-based catalyst is 150-200 nm, and the specific surface area is 200-300 m 2 The pore volume is 0.4-0.7 mL / g and the particle size is 30 mesh; the mass content of Ti is 0.35%, the molar ratio of silicon to titanium is 30:1, and the loading amount of rhodium is 0.1% of the total weight of the catalyst.

[0134] 3) Hydroformylation experiment:

[0135] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0136] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was increased to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0137] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0138] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 95.9% and the selectivity of the target product was 99.6%.

[0139] Example 5

[0140] 1) Preparation of titanium silicate molecular sieve TS-1 by hydrothermal method:

[0141] Same as Example 1.

[0142] 2) Preparation of rhodium-based catalyst using impregnation drying method:

[0143] 2-1) dispersing rhodium chloride in saturated ammonia water, adjusting the pH value to 7-10, and obtaining a 0.1 mol / L rhodium salt impregnation solution;

[0144] 2-2) adding the titanium silicon molecular sieve TS-1 to the impregnation solution, wherein the mass ratio of the impregnation solution to the titanium silicon molecular sieve is 70:1, and impregnating for 72 hours to obtain an impregnation mixture;

[0145] 2-3) filtering the impregnation mixture, drying at 80° C. for 10 h, heating to 500° C. at a rate of 10° C. / min, calcining for 4 h, and naturally cooling to room temperature to obtain a dry molecular sieve;

[0146] 2-4) adding sesbania powder, silica sol and liquid paraffin to the dry molecular sieve and mixing evenly, adding the mixture to an extruder for extrusion to obtain a rhodium-based catalyst; the mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:1.5:15:5.

[0147] The pore size of the rhodium-based catalyst is 120-170 nm, and the specific surface area is 350-450 m 2 The pore volume is 0.35-0.5 mL / g and the particle size is 38 mesh; the mass content of Ti is 0.35%, the molar ratio of silicon to titanium is 30:1, and the loading amount of rhodium is 0.1% of the total weight of the catalyst.

[0148] 3) Hydroformylation experiment:

[0149] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0150] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was increased to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0151] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0152] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 90.9% and the selectivity of the target product was 99.6%.

[0153] Example 6

[0154] Using the rhodium-based catalyst of Example 1, a hydroformylation experiment was carried out:

[0155] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0156] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was raised to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0157] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0158] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 98.5%, and the selectivity of the target product was 99.2%.

[0159] Example 7

[0160] Using the rhodium-based catalyst of Example 1, a hydroformylation experiment was carried out:

[0161] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0162] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:0.5. The temperature was raised to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0163] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0164] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 92.5%, and the selectivity of the target product was 98.3%.

[0165] Example 8

[0166] Using the rhodium-based catalyst of Example 1, a hydroformylation experiment was carried out:

[0167] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0168] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 200 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was raised to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0169] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0170] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 98.3%, and the selectivity of the target product was 98.8%.

[0171] Example 9

[0172] Using the rhodium-based catalyst of Example 1, a hydroformylation experiment was carried out:

[0173] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0174] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was raised to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0175] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0176] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 96.1%, and the selectivity of the target product was 99.3%.

[0177] Example 10

[0178] Using the rhodium-based catalyst of Example 1, a hydroformylation experiment was carried out:

[0179] 3-1) 1.7 g of titanium silicon molecular sieve rhodium catalyst was put into a 1 L high pressure reactor;

[0180] 3-2) Synthesis gas (CO and H2) was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was raised to 110°C at 10°C / h to stabilize the pressure at 7.0 MPa, and the reaction was continued for 10 hours.

[0181] 3-3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0182] The obtained reaction product was detected by gas chromatography, and the results showed that the conversion rate of the raw material isopentene was 98.7% and the selectivity of the target product was 99.0%.

[0183] Comparative Example 1

[0184] A method for preparing raw material isopentene comprises the following steps:

[0185] 1) 0.3 g of hydroxy(cyclooctadiene)rhodium dimer catalyst and 10.0 g of phosphite were put into a 1 L autoclave;

[0186] 2) Synthesis gas was charged into the reactor, and the pressure was maintained at 1.0 MPa. The reactor was replaced 4 times. 300 g of isopentene was injected into the reactor through a pressure tank, and then synthesis gas was charged, wherein the molar ratio of CO to H2 was 1:1. The temperature was raised to 110°C at 10°C / h to stabilize the pressure at 3.0 MPa, and the reaction was continued for 10 hours.

[0187] 3) After the reaction is completed, the system is cooled to room temperature naturally, and the reaction product is obtained by vacuum distillation.

[0188] The obtained reaction product is detected by gas chromatography, such as Figure 2 As shown, Figure 2 The gas chromatogram of the reaction product prepared in Comparative Example 1 of the present invention. Figure 2It can be seen that the conversion rate of the raw material isopentene is 89.7% and the selectivity of the target product is 97.4%.

[0189] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A rhodium-based catalyst comprising: Carrier and active ingredient; The carrier is TiOx-SiO2, and the active component is rhodium; In the rhodium-based catalyst, the loading amount of rhodium is 0.03% to 0.2% of the total weight of the catalyst.

2. The rhodium-based catalyst according to claim 1, characterized in that In the rhodium-based catalyst, the mass content of Ti is 0.3% to 0.5%, and the molar ratio of silicon to titanium is (25 to 45):

1.

3. The rhodium-based catalyst according to claim 1, characterized in that The pore size of the rhodium-based catalyst is 80-200 nm, and the specific surface area is 260-400 m 2 / g, pore volume is 0.3~0.5mL / g, and particle size is 10~80 mesh.

4. The method for preparing a rhodium-based catalyst according to any one of claims 1 to 3, comprising the following steps: S1) dispersing rhodium salt in saturated ammonia water, adjusting the pH value to 7 to 10, and obtaining an impregnation solution; S2) mixing the impregnation solution with titanium silicon molecular sieve TS-1 for impregnation to obtain an impregnation mixture; S3) filtering, drying, and calcining the impregnated mixture to obtain a dry molecular sieve; S4) mixing the dry molecular sieve, sesbania powder, silica sol and liquid paraffin, and shaping them to obtain a rhodium-based catalyst.

5. The preparation method according to claim 1, characterized in that: In step S1), the rhodium salt includes one or two of rhodium chloride, ammonium chlororhodate and chlororhodic acid; The rhodium salt is dispersed in a rhodium salt solution formed by ammonia water, and the concentration of rhodium is 0.002-0.4 mol / L.

6. The preparation method according to claim 1, characterized in that: In step S2), the mass ratio of the impregnation solution to the titanium silicon molecular sieve TS-1 is (50-100):1; The immersion time is 0.5 to 4 hours.

7. The preparation method according to claim 1, characterized in that: In step S3), after the drying, the step further includes: heating to a calcination temperature; the heating rate is 5 to 10°C / min; The calcination temperature is 400-600° C. and the calcination time is 4-8 hours.

8. The preparation method according to claim 1, characterized in that: In step S4), the solid content of the silica sol is 28% to 35%; The mass ratio of the dry molecular sieve, sesbania powder, silica sol and liquid paraffin is 100:1-3:10-40:5-10.

9. Use of the rhodium-based catalyst according to any one of claims 1 to 3 or the rhodium-based catalyst prepared by the preparation method according to any one of claims 4 to 8 as an isopentene hydroformylation catalyst.

10. The use according to claim 9, characterized in that: The reaction raw materials for isopentene hydroformylation include CO, H2 and isopentene; the reaction raw materials undergo isopentene hydroformylation reaction under the action of a rhodium-based catalyst; The molar ratio of CO to H2 is 0.1 to 2:1; The mass ratio of isopentene to the rhodium-containing catalyst is 200-450:0.5-4; The temperature of the hydroformylation reaction is 80-130° C., the time is 2-12 hours, and the pressure is 0.5-10 MPa.

Citation Information

Patent Citations

  • Method for preparing selective hydro-desulfurization catalyst

    CN102091651A

  • Precious metal modification method of titanium silicon molecular sieve

    CN103183357A

  • Titanium silicalite molecular sieve, synthetic method and application of titanium silicalite molecular sieve, and cyclic ketone oxidation method

    CN107879354A

  • Molded titanium silicalite molecular sieve containing precious metal and preparation method and application thereof, and method for producing hydrogen peroxide

    CN109574033A

  • Molecular sieve encapsulated rhodium heterogeneous core-shell catalyst for olefin hydroformylation, and catalytic method thereof

    CN109876847A

Cited By

  • Molecular sieve catalyst for encapsulating rhodium-based atom clusters as well as preparation method and application of molecular sieve catalyst

    CN122538261A