Desulfurization wastewater and coal-based solid waste coupling material as well as preparation method and application thereof

By mixing coal-based solid waste with desulfurization wastewater and adding modifiers, coupling materials suitable for backfill or soil improvement are prepared, which solves the problems of low utilization rate of coal-based solid waste and desulfurization wastewater treatment in the western region, and achieves efficient and economical Heavy metal removal and material utilization.

CN118926275AActive Publication Date: 2024-11-12CHINA ENERGY INVESTMENT CORP LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310519790.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The comprehensive utilization rate of coal-based solid waste in the western region is low, and the existing technology cannot effectively coordinate the treatment of desulfurization wastewater and fly ash, which cannot meet safety and economic requirements.

Method used

By mixing coal-based solid waste with desulfurization wastewater in a specific proportion and adding modifiers, including inorganic acids and soluble salts, reacting to prepare coupling materials, reducing the pH value and heavy metal content of coupling materials, forming suitable for backfill or soil improvement material.

Benefits of technology

The pH value of coal-based solid waste has been adjusted to 6-9, which significantly reduces the content of heavy metals and Se, meets the GB18599 and GB8978 standards, provides a coordinated treatment and utilization path of desulfurization wastewater and coal-based solid waste, and is simple in the process. Economical and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004220428180000101
    Figure BDA0004220428180000101
  • Figure BDA0004220428180000111
    Figure BDA0004220428180000111
  • Figure BDA0004220428180000112
    Figure BDA0004220428180000112
Patent Text Reader

Abstract

According to the desulfurization wastewater and coal-based solid waste coupling material and the preparation method and application thereof, the coupling material is prepared on the basis of desulfurization wastewater and coal-based solid waste through the method, and a new solution path is provided for cooperative treatment and subsequent utilization of desulfurization wastewater and coal-based solid waste. The preparation method comprises the following steps: 1) mixing and reacting 8-10 parts by weight of coal-based solid waste and 0.8-5.0 parts by weight of desulfurization wastewater; 2) mixing the mixed material obtained in the step 1) with 0.1-0.5 part by weight of a modifier to obtain a coupling material; wherein the pH value of the leachate of the coal-based solid waste used in the step 1) is greater than 9, the Se content is 0.1-0.5 mg / L, the pH value of the desulfurization wastewater used in the step 1) is 4-9, and the Mg ion content is greater than or equal to 50 mg / L; in the step (2), based on the total mass of the modifier, the modifier comprises 2-10% of inorganic acid and 90-98% of soluble salt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a desulfurization wastewater and coal-based solid waste treatment technology, and in particular to a desulfurization wastewater and coal-based solid waste coupling material, and a preparation method and application thereof. Background Art

[0002] Coal contains sulfur, and sulfur dioxide will be produced during the combustion of coal. At present, wet desulfurization is mainly used to treat sulfur-containing pollutants in power plant flue gas, producing desulfurization gypsum and desulfurization wastewater. On the other hand, a large amount of fly ash is produced during the combustion of coal, and the comprehensive utilization rate of fly ash in the central and eastern regions is greater than 70%. However, for the western region, on the one hand, the output of fly ash is huge; on the other hand, there are few ways to utilize it; due to the small capacity of the building materials market and the lack of comprehensive utilization methods for large-scale coal-based solid wastes, there is no large-scale market for fly ash consumption, which makes the comprehensive utilization rate of coal-based solid wastes in the western region significantly low, becoming a prominent problem restricting the development of the power industry. Ecological restoration applications such as backfilling and reclamation are effective ways to utilize large quantities of coal-based solid wastes, especially for the current market situation in the western region. However, the "GB18599-2020 General Industrial Solid Waste Storage and Landfill Pollution Control Standard" stipulates that only Class I industrial solid waste can be directly used as raw materials for backfilling or filling treatment in goafs. Most fly ash fails to meet the pH = 6-9 requirement due to its high alkalinity (pH greater than 9) and is difficult to use.

[0003] At present, there is still a lack of technology for the coordinated utilization of desulfurization wastewater and fly ash. Power plants use desulfurization wastewater mixed with fly ash to replace water that reduces dust during transportation, and finally use it as landfill. However, this method does not meet the requirements of the "GB18599-2020 General Industrial Solid Waste Storage and Landfill Pollution Control Standards" because it has not been harmlessly treated, and there are potential risks. The use of evaporation or crystallization water treatment technology is the safest and most reliable but most expensive treatment technology, which produces a small amount of high-salt water or concentrate, but it belongs to the scope of hazardous waste and still needs to be resolved.

[0004] Therefore, it is still necessary to explore solutions for the synergistic treatment of desulfurization wastewater and coal-based solid waste in order to balance economy, safety and reliability.

[0005] Chinese patent application CN202010366294.5 provides a zero-emission system for flue gas desulfurization wastewater, including a pretreatment unit, a concentration and reduction unit, a terminal solidification unit and a control system; the terminal solidification unit mixes the sedimentation slurry generated during the treatment of the desulfurization wastewater with fly ash, quicklime and silicate cement to form a low-grade building material; the mass percentage is sedimentation slurry: fly ash: quicklime: silicate cement = 1: (0.12-0.25): (0.15-0.3): (0.6-0.9). The present invention proposes a solution that is completely different from this solution. Summary of the invention

[0006] The present invention provides a method for preparing coupling materials of desulfurization wastewater and coal-based solid waste, as well as the coupling materials prepared and their applications. The method of the present invention is used to prepare coupling materials based on desulfurization wastewater and coal-based solid waste. On the one hand, it can solve the problem that the coal-based solidified material has a pH value greater than 9, which makes it difficult to utilize. On the other hand, compared with the initial coal-based solid waste and desulfurization wastewater, the obtained coupling material has a significantly reduced heavy metal content in the leaching liquid of the coupling material and has a lower Se content, which provides a new solution for the coordinated treatment and subsequent utilization of desulfurization wastewater and coal-based solid waste. Moreover, the method provided by the present invention has fewer process steps, a simple process, fewer types of reagents required, and does not require the input of additional water resources or heat energy, which is economical and environmentally friendly.

[0007] To achieve the purpose, the present invention provides the following technical solutions:

[0008] In one aspect, the present invention provides a method for preparing a coupling material of desulfurization wastewater and coal-based solid waste, the preparation method comprising the following steps:

[0009] 1) mixing 8-10 parts by weight of coal-based solid waste and 0.8-5.0 parts by weight of desulfurization wastewater to obtain a mixed material;

[0010] 2) mixing the mixed material obtained in step 1) with 0.1-0.5 parts by weight of a modifier to obtain the coupling material;

[0011] Wherein, the pH of the leaching solution of the coal-based solid waste used in step 1) is greater than 9, and the Se content is 0.1-0.5 mg / L;

[0012] The desulfurization wastewater used meets the following requirements: pH 4-9, Mg ion content ≥50mg / L;

[0013] In step 2), based on the total mass of the modifier, the modifier comprises 2-10% of inorganic acid and 90-98% of soluble salt; the soluble salt is selected from one or more of soluble aluminum salt and soluble iron salt, preferably soluble iron salt.

[0014] In the present invention, 8-10 parts by weight of the above-mentioned coal-based solid waste and 0.8-5.0 parts by weight of the above-mentioned desulfurization wastewater are first mixed and reacted, and then mixed with 0.1-0.5 parts by weight of a modifier of a specific composition to prepare a coupling material. This process does not need to be carried out in a system where a large amount of water exists. Through the above two-step reaction, the components interact with each other, not only can the high-alkali coal-based solid waste be modified to obtain a solid or semi-solid coupling material with a pH of 6-9 (measured by the leaching solution of the coupling material), but also can synergistically remove heavy metal pollutants in the desulfurization wastewater, and the heavy metal content in the leaching solution of the obtained coupling material is significantly reduced, and the Se content is greatly reduced. The obtained coupling material can be used as a mine filling or backfill material, soil reclamation or improvement material.

[0015] In the present invention, the modifier used includes 2-10% of inorganic acid and 90-98% of soluble salt, wherein the soluble salt is selected from soluble aluminum salt and / or soluble iron salt, and preferably, the inorganic acid is selected from at least one of sulfuric acid and hydrochloric acid. The inventors found that the mixed material obtained by reacting the modifier with coal-based solid waste and desulfurization wastewater is continuously contacted and reacted, and the obtained coupling material leachate not only has a pH of 6-9, but also the heavy metal content in the coupling material leachate is greatly reduced, and has a lower Se content.

[0016] In a preferred embodiment, the soluble salt used in the modifier is preferably a soluble iron salt. The inventors have found that the use of soluble iron salts is more beneficial to improving the treatment effect and further reducing the content of heavy metal ions in the leachate of the coupling material compared to the use of soluble aluminum salts.

[0017] In the present invention, the soluble iron salt and the soluble aluminum salt may be, for example, one or more of ferrous sulfate, ferric sulfate, ferric chloride, aluminum sulfate, aluminum chloride, and hydrates thereof.

[0018] In the present invention, if the soluble salt is a hydrate, its mass proportion in the modifier is 90-98%, which is measured only in the non-hydrated salt form corresponding to the soluble salt. For example, taking aluminum sulfate 18hydrate as an example, its mass proportion in the modifier is calculated as aluminum sulfate. In the present invention, the inorganic acid is preferably sulfuric acid or hydrochloric acid; the mass proportion of these two inorganic acids in the modifier is 2-10%, which is measured as H2SO4 in sulfuric acid and HCl in hydrochloric acid, respectively.

[0019] In the present invention, there is no particular restriction on the coal-based solid waste used. The coal-based solid waste is measured by its leachate, and the leachate satisfies pH>9 and Se content is 0.1-0.5 mg / L. The coupling material is prepared together with desulfurization wastewater according to the preparation method of the present invention. The obtained coupling material can better meet the requirements for reuse. For example, the pH of the leachate of the obtained coupling material can be reduced to 6-9, and it has a lower Se content, and the heavy metals in the leachate can be significantly removed. In some preferred embodiments, the coal-based solid waste in step 1) is selected from at least one of fly ash and bottom slag.

[0020] By adopting the method of the present invention, desulfurization wastewater with a pH of 4-9 and a Mg ion content of ≥50 mg / L and the above-mentioned coal-based solid waste are used to prepare coupling materials according to the preparation method of the present invention, and the heavy metal content in the leaching solution of the obtained coupling material can be greatly reduced, that is, it has a high heavy metal removal rate. In the present invention, there is no particular restriction on the source of the desulfurization wastewater used. In some embodiments, the desulfurization wastewater is selected from at least one of desulfurization wastewater raw water, desulfurization wastewater triple box effluent, and desulfurization wastewater concentrated water. In some embodiments, in step 1), the desulfurization wastewater used has a Cd content of 0.1-1 mg / L, a Cr content of 1.5-15 mg / L, a Cu content of 0.5-10 mg / L, a Ni content of 1-10 mg / L, and a Pb content of 1-10 mg / L.

[0021] In some preferred embodiments, the mixing reaction in step 1) includes: mixing the coal-based solid waste and desulfurization wastewater, and then standing to react for 8-24 hours; in step 2), standing for 1-7 days after mixing, and performing steps 1) and 2) according to the above preferred time range is conducive to the full interaction between the components, promoting the pH of the leachate of the obtained coupling material to reach 6-9, and is conducive to the reduction of heavy metal content and Se content.

[0022] The above-mentioned preparation method provided by the present invention is to pre-mix desulfurization wastewater and coal-based solid waste in a specific dosage range, and then continue to interact with a modifier of a specific composition in a specific dosage range. Through this process, the pain point of high Mg ion content in desulfurization wastewater can be converted into an advantage, making it an effective ion for modifying high-alkali coal-based solid waste, and modifying high-alkali fly ash through synergistic precipitation and inhibition. The pH of the leaching solution of the obtained coupling material can be reduced to 6-9, and the Se content can also be significantly reduced. At the same time, by utilizing the high alkalinity of coal-based solid waste, through the above-mentioned process, the heavy metal pollutants in the desulfurization wastewater can be synergistically removed in combination with the modifier. The heavy metal content of the leaching solution of the coupling material obtained after modification is significantly removed compared with the initial material, which can meet the requirements of GB8978.

[0023] By adopting the above-mentioned preparation method of the present invention, it is possible to solve the problem that the existing coal-based solid waste (such as fly ash and bottom ash) is difficult to further utilize because pH>9 and Se>0.1mg / L do not meet the requirements of GB 18599-2020 Class I industrial solid waste; it can also simultaneously transform the pain point of high Mg ion content in existing desulfurization wastewater into an advantage, as well as the risk of excessive heavy metal content, and provide a feasible technical route for zero discharge of desulfurization wastewater. By adopting the above-mentioned preparation method of the present invention, desulfurization wastewater and coal-based solid waste can be synergistically treated, and it is easy to prepare desulfurization wastewater and coal-based solid waste coupling materials that meet the GB18599 standard.

[0024] By adopting the above-mentioned preparation method of the present invention, the weight α3 of the heavy metal elements in the leaching solution of the obtained coupling material, the weight α1 of the heavy metal elements in the leaching solution of the coal-based solid waste used in step 1), and the weight α2 of the heavy metal elements in the desulfurization wastewater used in step 1) can satisfy the following relationship:

[0025] 40%≤((α1+α2-α3) / (α1+α2))×100%≤100%;

[0026] That is, the removal rate of heavy metal elements can reach 40%-100%, wherein the heavy metal elements include Cd, Cr, Cu, Ni and / or Pb.

[0027] Another aspect of the present invention is to provide a coupling material of desulfurized wastewater and coal-based solid waste prepared by the preparation method described above. The coupling material prepared by the preparation method of the present invention has a leachate pH of 6-9 and a Se content of ≤0.1 mg / L.

[0028] In the context of the present invention, the "leaching solution of coal-based solid waste" and "leaching solution of coupling material" involved in various places are obtained by leaching coal-based solid waste or coupling material with reference to HJ 557-2010 ("Horizontal Oscillation Method for Leaching Toxicity of Solid Waste"). The preparation of the leachate of coal-based solid waste is only to determine whether the coal-based solid waste used meets the requirements of the present invention, that is, the coal-based solid waste used is the corresponding coal-based solid waste with pH>9 and Se content of 0.1-0.5 mg / L obtained by the method in HJ 557-2010; it does not mean that the leachate is used in the preparation of the coupling material.

[0029] Another aspect of the present invention provides a method for synchronously treating desulfurized wastewater and coal-based solid waste, the method comprising: using the preparation method described above to prepare a coupling material from the desulfurized wastewater and coal-based solid waste, thereby achieving synchronous treatment of the desulfurized wastewater and coal-based solid waste;

[0030] Preferably, the coupling material is used for mine filling or backfilling, soil remediation or reclamation or improvement, ecological management, road materials, aggregates, mining materials, and / or trace metal element solidification; more preferably, it is used for mine filling or backfilling, soil reclamation or improvement.

[0031] On the other hand, the present invention also provides the application of the desulfurization wastewater and coal-based solid waste coupling material described above, and the coupling material is used in mine filling or backfilling, soil remediation or reclamation or improvement, ecological management, road materials, aggregates, mining materials, and / or trace metal element solidification; more preferably, it is used in mine filling or backfilling, soil reclamation or improvement.

[0032] The technical solution provided by the present invention has the following beneficial effects:

[0033] The coupling material preparation method provided by the present invention has a simple process, and the required reagents can prepare desulfurization wastewater and coal-based solid waste into coupling materials that are conducive to reuse without the need to invest additional water resources or heat energy. On the one hand, it can solve the problem that the coal-based solidified material is difficult to utilize due to its pH value greater than 9. On the other hand, compared with the initial coal-based solid waste and desulfurization wastewater, the obtained coupling material has a significantly reduced heavy metal content in the leaching solution of the coupling material and has a lower Se content, thereby providing a new solution path for the coordinated treatment and subsequent utilization of desulfurization wastewater and coal-based solid waste. DETAILED DESCRIPTION

[0034] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.

[0035] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0036] In the following text, "desulfurization wastewater and coal-based solid waste coupling materials" and "coupling materials" are the same concept, both referring to desulfurization wastewater and coal-based solid waste coupling materials.

[0037] In the following examples or comparative examples:

[0038] The leachate of coal-based solid waste and the leachate of coupling material were prepared according to HJ 557-2010 (Toxicity leaching method of solid waste - horizontal oscillation method).

[0039] The parameters of heavy metal element content and non-metallic element content were measured using the methods required by GB 8978-88 "Integrated Wastewater Discharge Standard".

[0040] The removal rate of each heavy metal element listed in Tables 1 and 2 is calculated according to the following formula:

[0041] ((α1+α2-α3) / (α1+α2))×100%

[0042] Among them, α1 refers to the weight of heavy metal elements in the leachate of coal-based solid waste used to prepare the coupling material, in mg; α2 refers to the weight of heavy metal elements in desulfurization wastewater used to prepare the coupling material, in mg; α3 refers to the weight of heavy metal elements in the leachate of the prepared coupling material, in mg.

[0043] In order to facilitate understanding of the calculation process of the removal rate of the heavy metal elements, the removal rate of the Cr element in Example 1 is used as an example for explanation below:

[0044] According to the formula of Example 1 (8 parts by weight of fly ash, 5.0 parts by weight of desulfurization wastewater, 0.1 parts by weight of modifier), 100.00g of fly ash on a dry basis corresponds to 62.50g of desulfurization wastewater (volume 62.50ml), and the modifier is 1.25g; the final coupling material obtained has a dry basis weight of 100.00g. 100.00g of fly ash on a dry basis from the same batch as Example 1 was made into a leachate (volume 1L), and the content of heavy metal element Cr in the leachate was measured to be 0.10mg / L. By multiplying this content by the volume of the leachate, the weight of the Cr element in the coal-based solid waste used can be obtained to be 0.10mg (i.e., the α1 value in the formula). The content of heavy metal element Cr in the same batch of desulfurization wastewater as in Example 1 is 15.00 mg / L. By multiplying this content by the volume of desulfurization wastewater used in Example 1 (62.50 ml), the weight of heavy metal element Cr in desulfurization wastewater is 0.94 mg (i.e., α2 value). 100.00 g of the coupling material obtained in Example 1 with a dry basis weight is made into a leachate (with a volume of 1 L). The content of heavy metal element Cr in the leachate is measured to be 0 mg / L. By multiplying this content by the volume of the leachate, the weight of Cr element in the coupling material is 0 mg (i.e., α3 value in the formula).

[0045] The removal rate of the Cr element in Example 1 is calculated according to the following formula: ((α1+α2-α3) / (α1+α2))×100%, substituting the above-obtained α1, α2, and α3 values ​​for calculation, ((0.1+0.94-0) / (0.1+0.94))×100%=100%, that is, in Example 1, the removal rate of the Cr element is 100%.

[0046] The calculation of the heavy metal content in the remaining embodiments and comparative examples refers to the above process and will not be repeated here.

[0047] Ingredients Description:

[0048] The desulfurization wastewater used in the examples and comparative examples has a pH of 4-9 and a Mg ion content of ≥50 mg / L. In the desulfurization wastewater, the Cd content is 0.1-1 mg / L, the Cr content is 1.5-15 mg / L, the Cu content is 0.5-10 mg / L, the Ni content is 1-10 mg / L, and the Pb content is 1-10 mg / L.

[0049] The fly ash used in the examples and comparative examples has a leaching solution with a pH value greater than 9 and a Se content of 0.1-0.5 mg / L.

[0050] The bottom slag used in the examples has a leaching solution with a pH value of >9 and a Se content of 0.1-0.5 mg / L.

[0051] Examples 1-6

[0052] Examples 1-6 all prepare desulfurization wastewater and coal-based solid waste coupling materials according to the following steps:

[0053] 1) Mixing coal-based solid waste and desulfurization wastewater, and allowing to react for a period of time (for specific reaction time, see Table 1 below) to obtain a mixed material;

[0054] 2) The mixed material obtained in step 1) is mixed with a modifier and allowed to stand for a period of time (for specific standing time, see Table 1 below) to obtain a coupling material.

[0055] The weight parts of coal-based solid waste, desulfurization wastewater, modifier, and the composition of the modifier used are all shown in Table 1.

[0056] Example 7

[0057] The method is carried out in accordance with Example 1, except that the soluble salt used is a soluble aluminum salt (aluminum sulfate 18hydrate).

[0058] Comparative Example 1-1

[0059] The same steps are described in Example 1, except that the amount of the modifier is adjusted to 1 part by weight.

[0060] Comparative Example 1-2

[0061] The same steps are described in reference to Example 1, except that the amount of the modifier is reduced to 0.05 parts by weight.

[0062] Comparative Example 2-1

[0063] The same method is carried out with reference to Example 1, except that the amount of fly ash is adjusted to 15 parts by weight.

[0064] Comparative Example 2-2

[0065] The same method is carried out with reference to Example 1, except that the amount of fly ash is adjusted to 5 parts by weight.

[0066] Comparative Example 3

[0067] The process is carried out in accordance with Example 1, except that no desulfurization wastewater is used in step 1).

[0068] Comparative Example 4

[0069] The method is carried out in accordance with Example 1, except that, in the modifier, the proportion of inorganic acid is 15 wt %, and the proportion of soluble salt is 85 wt %.

[0070] Comparative Example 5

[0071] The method is carried out in accordance with Example 1, except that, in the modifier, the proportion of inorganic acid is 1.5 wt %, and the proportion of soluble salt is 98.5 wt %.

[0072] Comparative Example 6

[0073] The method is carried out in accordance with Example 1, except that the coal-based solid waste, desulfurization wastewater and modifier are directly mixed at the same time in one step and allowed to react for 8 days.

[0074] Table 1

[0075]

[0076]

[0077] Table 2

[0078]

[0079]

[0080] It can be seen from the experimental results of Examples 1-7 that the process of the present invention is used to synergistically treat desulfurization wastewater and coal-based solid waste, and the two are used to prepare a coupling material through a two-step method. The leaching solution of the obtained coupling material meets the pH requirement of 6-9, and the heavy metal removal rate is obvious, and the Se content is significantly reduced, which can meet the subsequent utilization requirements, for example, it can be used as mine filling, backfill material, soil reclamation material or soil improvement material.

[0081] From the experimental comparison of Examples 1-6 and Example 7, it can be seen that under the same conditions, the Se content in the leaching solution of the coupling material obtained by using soluble iron salt is lower than that by using soluble aluminum salt, and the removal rate of heavy metal elements is higher.

[0082] Compared with the embodiments of the present invention, each comparative example does not adopt the process requirements of the present invention to prepare the coupling material. As a result, the leaching solution of the obtained coupling material cannot meet the pH requirement of 6-9, and the Se content is significantly higher than the results of the embodiments.

[0083] From the experimental comparison of the examples of the present application and the comparative examples, it can be seen that the formulation system of the present invention is used to prepare coupling materials based on coal-based solid waste and desulfurization wastewater, which can well take into account the following effects: 1) the obtained coupling material leachate meets the pH requirement of 6-9, 2) lower Se content in the leachate, and 3) good simultaneous removal effect of multiple heavy metal elements. However, it is difficult to well take into account the above effects in the comparative examples.

[0084] In Examples 1-7 of the present invention, the obtained leaching solutions of the coupling materials were tested and found to meet the GB18599 standard, and the heavy metal content thereof met the requirements of GB8978.

[0085] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.

Claims

1. A method for preparing a coupling material of desulfurization wastewater and coal-based solid waste, characterized in that: The preparation method comprises the following steps: 1) mixing 8-10 parts by weight of coal-based solid waste and 0.8-5.0 parts by weight of desulfurization wastewater to obtain a mixed material; 2) mixing the mixed material obtained in step 1) with 0.1-0.5 parts by weight of a modifier to obtain the coupling material; Wherein, the pH of the leaching solution of the coal-based solid waste used in step 1) is greater than 9, and the Se content is 0.1-0.5 mg / L; The desulfurization wastewater used meets the following requirements: pH 4-9, Mg ion content ≥50mg / L; In step 2), based on the total mass of the modifier, the modifier comprises 2-10% of inorganic acid and 90-98% of soluble salt; the soluble salt is selected from one or more of soluble aluminum salt and soluble iron salt, preferably soluble iron salt.

2. The preparation method according to claim 1, characterized in that: The inorganic acid is selected from at least one of sulfuric acid and hydrochloric acid.

3. The preparation method according to claim 1, characterized in that: The coal-based solid waste in step 1) is selected from at least one of fly ash and bottom slag.

4. The preparation method according to claim 1, characterized in that: The desulfurization wastewater is selected from at least one of desulfurization wastewater raw water, desulfurization wastewater triple tank effluent, and desulfurization wastewater concentrated water.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step 1), the desulfurization wastewater used has a Cd content of 0.1-1 mg / L, a Cr content of 1.5-15 mg / L, a Cu content of 0.5-10 mg / L, a Ni content of 1-10 mg / L, and a Pb content of 1-10 mg / L.

6. The preparation method according to any one of claims 1 to 4, characterized in that: The mixing reaction in step 1) comprises: mixing the coal-based solid waste and the desulfurization wastewater, and then standing to react for 8-24 hours; in step 2), standing to react for 1-7 days after mixing.

7. A desulfurization wastewater and coal-based solid waste coupling material prepared according to the preparation method according to any one of claims 1 to 6.

8. The desulfurization wastewater and coal-based solid waste coupling material according to claim 7, characterized in that: The pH of the leaching solution of the coupling material is 6-9, and the Se content is ≤0.1 mg / L.

9. A method for simultaneous treatment of desulfurization wastewater and coal-based solid waste, characterized in that: The synchronous treatment method comprises: using the preparation method according to any one of claims 1 to 6 to prepare a coupling material from the desulfurization wastewater and coal-based solid waste; Preferably, the coupling material is used for mine filling or backfilling, soil remediation or reclamation or improvement, ecological management, road materials, aggregates, mining materials, and / or trace metal element solidification; more preferably, it is used for mine filling or backfilling, soil reclamation or improvement.

10. The use of the desulfurization wastewater and coal-based solid waste coupling material according to claim 8, characterized in that: The coupling material is used in mine filling or backfilling, soil remediation or reclamation or improvement, ecological management, road materials, aggregates, mining materials, and / or trace metal element solidification; more preferably, it is used in mine filling or backfilling, soil reclamation or improvement.

Citation Information

Patent Citations

  • Method of co-treating solidified heavy metal with fly ash and desulfurization wastewater

    CN110040809A

  • Hazardous waste incineration wet deacidification and fly ash washing co-processing method and system

    CN113401923A

  • Cooperative treatment method for magnesium desulfurization wastewater and garbage fly ash

    CN115371049A

  • Zero-discharge and resourceful treatment process for fly ash wastewater

    CN115745309A

  • Wastewater Disposal Method in Flue Gas DesulfurizationSystem by Using Scale Preventer

    KR1020060001283A