Aluminum alloy conductor and preparation method thereof

By adjusting the composition and process of aluminum alloy material, using online induction heating and three-stage annealing process, the problem of insufficient conductivity and tensile strength of existing aluminum alloy wires is solved, and the conductivity and heat resistance is significantly improved, which meets the A wider application requirement.

CN118926345APending Publication Date: 2024-11-12JIANGSU HENGTONG ELECTRICAL SPECIAL WIRE CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411003926.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In mass production, the single wire performance is insufficient, the conductivity and tensile strength are low, and the composition and process are unreasonable, resulting in uneven distribution of the Zr-containing phase of the microalloy and incomplete precipitation, which makes it difficult to Meet more application needs.

Method used

By adjusting the chemical composition and production process of aluminum alloy materials, online induction heating and three-stage annealing process are adopted, and phased refining is used using aluminum-boron intermediate alloy, aluminum-zirconium intermediate alloy, aluminum-erbium intermediate alloy, etc., and combined with different refining agents and gases for refining Impurities removal improve conductivity and heat resistance.

Benefits of technology

The conductivity and tensile strength of aluminum alloy wires are significantly improved, with conductivity reaching 62.5% IACS, heat resistance reaching 95%, and tensile strength of 220MPa-260MPa, meeting the wider application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962441110000081
    Figure BDA0004962441110000081
Patent Text Reader

Abstract

The invention relates to an aluminum alloy conductor and a preparation method thereof, and belongs to the technical field of aluminum alloy materials. The preparation method comprises the following steps: S1, melting an aluminum ingot, and adding an aluminum-boron intermediate alloy for refining to obtain first molten aluminum; s2, an aluminum-zirconium intermediate alloy is added into the first molten aluminum to be evenly stirred, and second molten aluminum is obtained; s3, an aluminum-erbium intermediate alloy, an aluminum-neodymium intermediate alloy and an aluminum-praseodymium intermediate alloy are added into the first molten aluminum for staged refining, and third molten aluminum is obtained; s4, degassing and deslagging are conducted on the third molten aluminum, and fourth molten aluminum is obtained; and S5, the fourth molten aluminum is subjected to continuous casting, induction heating, rolling, annealing and cold drawing, and the aluminum alloy wire is obtained. The electric conductivity and the heat resistance of the aluminum alloy conductor are improved by adjusting the chemical components of the aluminum alloy material, improving the production process, increasing the casting temperature, using an online induction heating process and matching with a three-section annealing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy materials, and in particular relates to an aluminum alloy wire and a preparation method thereof. Background Art

[0002] Super heat-resistant aluminum alloy conductors can operate at 210°C for a long time and 240°C for a short time due to their high temperature and high pressure resistance. They are widely used in long-distance UHV transmission lines such as West-East Power Transmission, and are also gradually being used in solar and wind power generation fields with extreme climates and intermittent unstable power generation. However, most of the current super heat-resistant aluminum alloy conductors still have many deficiencies in the performance of single wires in actual mass production.

[0003] Chinese invention patent CN116716498A discloses a high-conductivity super-heat-resistant aluminum alloy material and a preparation method thereof, which prepares a heat-resistant aluminum alloy material with a conductivity of 61.8% IACS-62.1% IACS, a heat resistance of 96%-98%, and a tensile strength of 170MPa-200MPa. However, in this method, Zr, Y, and Er are used to form a strengthening phase, and the tensile strength and synergistic precipitation ability are low, and the composition-process matching is unreasonable, resulting in uneven distribution of the micro-alloyed Zr-containing phase and incomplete precipitation, making it difficult to mass-produce high-performance materials / wires.

[0004] Therefore, a new method is urgently needed to improve the electrical conductivity and tensile strength of aluminum alloy wires to meet more application requirements. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an aluminum alloy wire and a preparation method thereof, which improves the conductivity and heat resistance of the aluminum alloy wire by adjusting the chemical composition of the aluminum alloy material and improving the production process, increasing the casting temperature, using an online induction heating process, and combining a three-stage annealing process.

[0006] The first object of the present invention is to provide a method for preparing an aluminum alloy wire, comprising the following steps:

[0007] S1, melting the aluminum ingot, adding aluminum-boron master alloy for refining, and obtaining the first aluminum liquid;

[0008] S2, adding aluminum-zirconium master alloy to the first aluminum liquid described in S1 and stirring evenly to obtain a second aluminum liquid;

[0009] S3, adding an aluminum-erbium master alloy, an aluminum-neodymium master alloy and an aluminum-praseodymium master alloy to the first aluminum liquid described in S2 for stage-by-stage refining to obtain a third aluminum liquid;

[0010] S4, degassing and deslagging the third aluminum liquid described in S3 to obtain a fourth aluminum liquid;

[0011] S5. Continuously casting, induction heating, rolling, annealing and cold drawing the fourth aluminum liquid described in S4 to obtain an aluminum alloy wire.

[0012] In one embodiment of the present invention, the chemical composition and mass percentage of the aluminum alloy material are: Si 0-0.03%, Fe 0-0.06%, Zr 0.5%-0.9%, Er 2.0%-3.0%, Nd 0.5%-1.0%, Pr0.3%-0.7%, B 0-0.0005%, the sum of Cr, Mn, V and Ti is 0-0.0005%, and the balance is Al and other inevitable impurities.

[0013] In one embodiment of the present invention, in S1, the melting temperature is 800°C-850°C;

[0014] And / or, the refining is performed under the conditions of nitrogen and a granular refining agent for 20 min-30 min, and then left to stand for 20 min-30 min.

[0015] In one embodiment of the present invention, in S2, the stirring is carried out under nitrogen for 10 min to 20 min, and then allowed to stand for 10 min to 20 min.

[0016] In one embodiment of the present invention, in S3, the staged refining includes primary refining and secondary refining; the primary refining is performed under nitrogen and a granular refining agent at 800°C-850°C for 20min-30min, and then allowed to stand for 10min-20min; the secondary refining is performed under argon and a sodium-free refining agent at 800°C-850°C for 20min-30min, and then allowed to stand for 40min-60min.

[0017] In one embodiment of the present invention, in S5, the process parameters of the continuous casting are: the casting temperature is 740℃-770℃, the casting speed is 4t / h-5t / h, the cooling water temperature of the front end zone is 10℃-20℃, the cooling water temperature of the remaining areas is 25℃-35℃, and the billet outlet temperature is 450℃-500℃.

[0018] In one embodiment of the present invention, in S5, the temperature of the induction heating is 580°C-630°C.

[0019] In one embodiment of the present invention, in S5, the rolling process parameters are: nominal diameter is 14.5mm-15.5mm, rolling temperature is 580℃-630℃, final rolling temperature is 300℃-400℃, and winding temperature is 250℃-300℃.

[0020] In one embodiment of the present invention, in S5, the annealing is divided into three stages, the first stage is annealing at 320℃-360℃ for 10h-30h, the second stage is annealing at 430℃-480℃ for 40h-100h, and the third stage is cooling to below 300℃ within 3h-10h.

[0021] In one embodiment of the present invention, the chemical composition of the particulate refining agent is an anhydrous granular molten salt synthetic mixture, which can effectively remove various alkali metals (such as sodium, calcium and lithium), non-metallic inclusions, oxides, carbides and borides, etc. that fall off from electrolytic aluminum liquid, aluminum alloy liquid and furnace refractory lining.

[0022] In one embodiment of the present invention, the chemical composition of the sodium-free refining agent is fluorides such as calcium fluoride and potassium fluorosilicate and chlorides such as potassium chloride.

[0023] The second object of the present invention is to provide an aluminum alloy wire prepared by the method.

[0024] The technical solution of the present invention has the following advantages over the prior art:

[0025] (1) The preparation method of the present invention performs boronization treatment on the aluminum-boron master alloy, so that the B element reacts more completely with the impurity elements such as Cr, Mn, V, and Ti, thereby reducing the content of impurity elements in the aluminum melt and improving the conductivity. By using the BV and Zr-B chemical reactions, the operations of adding B to reduce V and adding Zr to reduce B are performed successively, so that the content of impurity elements is lower and the electrical properties are improved.

[0026] (2) The preparation method described in the present invention uses different refining agents (granular refining agent and sodium-free refining agent) and refining gases in different steps to remove different impurities in steps and save material costs. Nitrogen and granular refining agents are used in the preparation of the first aluminum liquid. The granular refining agent has a long reaction time with the aluminum melt. When the granular refining agent is left standing in the furnace, it can fully react with the aluminum melt to remove the alkali metal and non-metallic oxide inclusions in the aluminum melt. In order to improve the purity of the aluminum liquid during the preparation of the third aluminum liquid, granular refining agents and sodium-free refining agents are used for staged refining to avoid the formation of low-melting-point eutectics by sodium elements. Structural defects will occur during the casting and annealing processes. Nitrogen and argon are used for refining to enhance the dehydrogenation effect. The hydrogen atoms in the aluminum melt gather to form hollows during casting, which affects the mechanical and electrical properties.

[0027] (3) The continuous casting process adopted in the preparation method described in the present invention adopts an extremely high casting temperature and part of low-temperature cooling water to ensure that the supersaturated Zr element in the aluminum liquid forms a metastable dispersed phase Al3Zr (L12) rather than a primary Al3Zr phase during casting. Therefore, the Al3Zr (L12) phase can be transformed by heat treatment, greatly improving the conductivity; a short online high-temperature solid solution is beneficial to the subsequent heat treatment to precipitate the Zr, Er, Nd, and Pr elements.

[0028] (4) The preparation method described in the present invention adopts a staged annealing process. In the first stage, Er, Nd, and Pr are rapidly precipitated at the grain boundary. In the second stage, Zr begins to precipitate, and uses the Al3 (Er, Nd, Pr) phase precipitated in the first stage as the nucleus to precipitate rapidly and thoroughly, thereby greatly reducing the resistivity.

[0029] (5) The aluminum alloy wire described in the present invention is produced using aluminum ingots with low Si and low Fe. The negative effects of these two elements on electrical properties are far greater than their positive effects on heat resistance. Therefore, compared with other super heat-resistant aluminum alloy materials, higher conductivity can be achieved; Zr element can inhibit the recrystallization growth of crystal structure, thereby improving the heat resistance of the material. However, Zr element dissolved in the aluminum matrix has a great influence on resistivity. Therefore, Zr element is converted into precipitated Al3Zr through heat treatment, thereby improving the conductivity of the material; Er and Nd elements precipitate Al3 (Er, Nd, Zr) phase through heat treatment, pinned at the grain boundary, hindering grain growth, and improving tensile strength and heat resistance; Pr element rare earth optimization acts on impurity elements to form spheroidized phase, improving electrical properties and tensile strength, and also forms compounds with Zr together with Er and Nd elements, pinned at the grain boundary, and improving heat resistance. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0031] Example 1

[0032] The aluminum alloy wire and the preparation method thereof of the present embodiment specifically include the following steps:

[0033] S1. Add an aluminum ingot with a purity of 99.85% into a No. 1 smelting furnace and heat it to melt at 825°C, add aluminum-boron master alloy particles at a rate of 2 kg per ton for boronization, and use a fully automatic refining vehicle to blow in nitrogen and particle refining agent for refining for 25 minutes, then let it stand for 25 minutes and then skim the slag to obtain the first aluminum liquid;

[0034] S2, transferring the first aluminum liquid to the No. 2 smelting furnace, adding 3 kg / ton of aluminum-zirconium master alloy, then using a fully automatic refining vehicle to blow nitrogen and stir for 15 minutes, then standing for 15 minutes to obtain the second aluminum liquid;

[0035] S3, the second aluminum liquid is poured into a holding furnace, and aluminum-erbium master alloy, aluminum-neodymium master alloy and aluminum-praseodymium master alloy are added, and argon gas and granular refining agent are blown into the furnace for primary refining at 825°C for 25 minutes using a fully automatic refining car, and the surface scum is removed after standing for 15 minutes, and argon gas and sodium-free refining agent are blown into the furnace for secondary refining at 825°C for 25 minutes using a fully automatic refining car, and the surface scum is removed after standing for 15 minutes, and the third aluminum liquid is obtained after standing for 35 minutes;

[0036] S4, the third aluminum liquid in the holding furnace is poured into the launder, and the aluminum liquid is degassed and deslagging through a double-rotor online degassing box and a tubular filter box to obtain a fourth aluminum liquid having a chemical composition and a mass percentage of Si 0.025%, Fe 0.042%, Zr 0.62%, Er 2.4%, Nd 0.88%, Pr 0.54%, B 0.0002%, Cr+Mn+V+Ti0.0003%;

[0037] S5, continuously casting the fourth aluminum liquid to obtain a low-temperature ingot; wherein the casting temperature is 765°C, the casting speed is 4.5t / h, the cooling water temperature of the front zone is 18°C, the cooling water temperature of the remaining zones is 30°C, and the ingot outlet temperature is 470°C;

[0038] S6, performing online induction heating on the low temperature cast billet to obtain a continuous billet with a temperature of 605° C.;

[0039] S7, rolling the continuous billet to obtain an aluminum rod; wherein the nominal diameter is 15 mm, the feed rolling temperature is 605° C., the final rolling temperature is 350° C., and the rod closing temperature is 270° C.;

[0040] S8, using a heat treatment furnace to anneal the aluminum rod in stages, the first stage is annealing at 340°C for 20 hours, the second stage is annealing at 450°C for 65 hours, and the third stage is heating stopped, the furnace is cooled to 270°C within 8 hours, and then the aluminum wire is obtained;

[0041] S9, cold draw the aluminum wire, and draw it through 8 passes. The thickness of the aluminum alloy wire is 3.5 mm.

[0042] Example 2

[0043] The aluminum alloy wire and the preparation method thereof of the present embodiment specifically include the following steps:

[0044] S1. Add an aluminum ingot with a purity of 99.999% into a No. 1 smelting furnace and heat it to melt at 825°C, add 0.8 kg / ton of aluminum-boron master alloy particles for boronization, and use a fully automatic refining vehicle to blow in nitrogen and a particle refining agent for refining for 25 minutes, then let it stand for 25 minutes and then skim the slag to obtain the first aluminum liquid;

[0045] S2, transferring the first aluminum liquid to the No. 2 smelting furnace, adding 1.2 kg / ton of aluminum-zirconium master alloy, then using a fully automatic refining vehicle to blow nitrogen and stir for 15 minutes, then standing for 15 minutes to obtain the second aluminum liquid;

[0046] S3, the second aluminum liquid is poured into a holding furnace, and aluminum-erbium master alloy, aluminum-neodymium master alloy and aluminum-praseodymium master alloy are added, and argon gas and granular refining agent are blown into the furnace for primary refining at 825°C for 25 minutes using a fully automatic refining car, and the surface scum is removed after standing for 15 minutes, and argon gas and sodium-free refining agent are blown into the furnace for secondary refining at 825°C for 25 minutes using a fully automatic refining car, and the surface scum is removed after standing for 15 minutes, and the third aluminum liquid is obtained after standing for 35 minutes;

[0047] S4, the third aluminum liquid in the holding furnace is poured into the launder, and the aluminum liquid is degassed and deslagging through a double-rotor online degassing box and a tubular filter box to obtain a fourth aluminum liquid with chemical composition and mass percentage of Si 0.011%, Fe 0.023%, Zr 0.88%, Er 2.9%, Nd 1.0%, Pr 0.7%, B 0.0002%, Cr+Mn+V+Ti 0.0001%;

[0048] S5, continuously casting the fourth aluminum liquid to obtain a low-temperature ingot; wherein the casting temperature is 770°C, the casting speed is 4.8 t / h, the cooling water temperature of the front end zone is 20°C, the cooling water temperature of the remaining zones is 33°C, and the ingot outlet temperature is 491°C;

[0049] S6, performing online induction heating on the low temperature cast billet to obtain a continuous billet with a temperature of 621° C.;

[0050] S7, rolling the continuous billet to obtain an aluminum rod; wherein the nominal diameter is 15 mm, the feed rolling temperature is 621° C., the final rolling temperature is 350° C., and the rod closing temperature is 300° C.;

[0051] S8, using a heat treatment furnace to anneal the aluminum rod in stages, the first stage is annealing at 360° C. for 12 hours, the second stage is annealing at 470° C. for 40 hours, and the third stage is heating stopped, and the furnace is cooled to 240° C. within 10 hours to obtain an aluminum wire;

[0052] S9, cold draw the aluminum wire, and draw it through 10 passes. The thickness of the aluminum alloy wire is 3.5 mm.

[0053] Example 3

[0054] The aluminum alloy wire and the preparation method thereof of the present embodiment specifically include the following steps:

[0055] S1. Add an aluminum ingot with a purity of 99.85% into a No. 1 smelting furnace and heat it to melt at 825°C, add aluminum-boron master alloy particles at a rate of 8 kg per ton for boronization, and use a fully automatic refining vehicle to blow in nitrogen and particle refining agent for refining for 25 minutes, then let it stand for 25 minutes and then skim the slag to obtain the first aluminum liquid;

[0056] S2, transferring the first aluminum liquid to the No. 2 smelting furnace, adding 3 kg / ton of aluminum-zirconium master alloy, then using a fully automatic refining vehicle to blow nitrogen and stir for 15 minutes, then standing for 15 minutes to obtain the second aluminum liquid;

[0057] S3, the second aluminum liquid is poured into a holding furnace, and aluminum-erbium master alloy, aluminum-neodymium master alloy and aluminum-praseodymium master alloy are added, and argon gas and granular refining agent are blown into the furnace for primary refining at 825°C for 25 minutes using a fully automatic refining car, and the surface scum is removed after standing for 15 minutes, and argon gas and sodium-free refining agent are blown into the furnace for secondary refining at 825°C for 25 minutes using a fully automatic refining car, and the surface scum is removed after standing for 15 minutes, and the third aluminum liquid is obtained after standing for 35 minutes;

[0058] S4, the third aluminum liquid in the holding furnace is poured into the launder, and the aluminum liquid is degassed and deslagging through a double-rotor online degassing box and a tubular filter box to obtain a fourth aluminum liquid with chemical composition and mass percentage of Si 0.028%, Fe 0.054%, Zr 0.51%, Er 2.0%, Nd 0.5%, Pr 0.4%, B 0.0003%, Cr+Mn+V+Ti 0.0002%;

[0059] S5, continuously casting the fourth aluminum liquid to obtain a low-temperature ingot; wherein the casting temperature is 744°C, the casting speed is 4.1t / h, the cooling water temperature of the front zone is 14°C, the cooling water temperature of the remaining zones is 28°C, and the ingot outlet temperature is 455°C;

[0060] S6, performing online induction heating on the low temperature cast billet to obtain a continuous billet with a temperature of 588° C.;

[0061] S7, rolling the continuous billet to obtain an aluminum rod; wherein the nominal diameter is 15 mm, the feed rolling temperature is 588° C., the final rolling temperature is 350° C., and the rod closing temperature is 250° C.;

[0062] S8, using a heat treatment furnace to anneal the aluminum rod in stages, the first stage is annealing at 320° C. for 30 hours, the second stage is annealing at 435° C. for 95 hours, and the third stage is heating stopped, and the furnace is cooled to 280° C. within 3 hours to obtain an aluminum wire;

[0063] S9, cold draw the aluminum wire, and draw it through 6 passes. The thickness of the aluminum alloy wire is 4.2 mm.

[0064] Comparative Example 1

[0065] It is basically the same as Example 1, except that the mass percentage of Si is 0.05%.

[0066] Comparative Example 2

[0067] The method is basically the same as Example 1, except that no Zr is added.

[0068] Comparative Example 3

[0069] The same as embodiment 1, except that Er is not added.

[0070] Comparative Example 4

[0071] It is basically the same as Example 1, except that no Nd is added.

[0072] Comparative Example 5

[0073] The method is basically the same as Example 1, except that Pr is not added.

[0074] Comparative Example 6

[0075] It is basically the same as Example 1, except that Nd and Pr are not added.

[0076] Comparative Example 7

[0077] The method is basically the same as Example 1, except that Er, Nd and Pr are not added.

[0078] Comparative Example 8

[0079] The method is basically the same as Example 1, except that only the first stage annealing is used.

[0080] Comparative Example 9

[0081] The method is basically the same as Example 1, except that the third stage annealing is not used.

[0082] Comparative Example 10

[0083] The method is basically the same as Example 1, except that the cooling water temperature in the front end zone is 30°C.

[0084] Test Case

[0085] The aluminum alloy wires prepared in Examples 1-3 and Comparative Examples 1-10 were tested for properties such as tensile strength:

[0086] Tensile strength and elongation at break: measured in accordance with GB / T 4909.3 "Bare wire test methods Part 3: Tensile test";

[0087] Conductivity: Determined in accordance with GB / T 3048.2 "Electrical performance test methods for wires and cables Part 2: Resistivity test of metallic materials";

[0088] Heat resistance: Determined in accordance with the standard "GB / T 30551-2014 Heat-resistant aluminum alloy wire for overhead stranded wire";

[0089] Table 1 shows the relevant properties of the aluminum alloy conductor finally measured:

[0090] Table 1

[0091]

[0092] It can be seen from Table 1 that the electrical conductivity of the aluminum alloy wire prepared in the embodiment reaches 62.5% IACS, the heat resistance reaches 95%, and the tensile strength is 220 MPa-260 MPa.

[0093] By comparing Example 1 and Comparative Examples 1-7, it can be seen that the composition and content of elements will affect the performance of aluminum alloy wires. Zr is the main element that provides heat resistance in aluminum alloy wires, forming Al3Zr, which is pinned between grains, thereby improving heat resistance and reducing conductivity; conversely, when Zr is absent, conductivity is improved, but heat resistance is lost. Er, Nd, and Pr elements precipitate during the annealing process, and Zr element uses this precipitation structure as a crystal nucleus to precipitate faster and more fully, thereby improving conductivity. Although the Y element has a similar effect to the above elements, the performance of Er, Nd, and Pr is improved by adding a specific combination of composition, production process, and annealing process. However, the Y element is not as good as Er, Nd, and Pr in its ability to precipitate at one time, and Al3Zr cannot be further precipitated as Al3Y better, so the strength and electrical properties of the comparative example are far inferior to those of the embodiment;

[0094] By comparing Example 1 with Comparative Examples 8-9, it can be seen that the annealing process affects the performance of the aluminum alloy wire. The first stage of annealing is mainly for the precipitation of Er, Nd, and Pr, and the second stage is for the precipitation of Zr. In addition, the crystal nuclei of the precipitation organization are quickly and fully precipitated in the first stage. In the comparative example, a certain annealing stage is missing, and the precipitation of Er, Nd, PrZr is incomplete, and the electrical properties are poor.

[0095] By comparing Example 1 and Comparative Example 10, it can be seen that the cooling water temperature in the front zone affects the performance of the aluminum alloy wire. Heat cannot be quickly exchanged in the initial stage of solidification, forming a primary Al3Zr phase, which cannot be eliminated after annealing, resulting in poor electrical properties. In addition, a large number of cracks, fissures, and even fractures appear in the billet, making it impossible to produce in batches continuously.

[0096] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing an aluminum alloy wire, characterized in that: The following steps are involved: S1, melting the aluminum ingot, adding aluminum-boron master alloy for refining, and obtaining the first aluminum liquid; S2, adding aluminum-zirconium master alloy to the first aluminum liquid described in S1 and stirring evenly to obtain a second aluminum liquid; S3, adding an aluminum-erbium master alloy, an aluminum-neodymium master alloy and an aluminum-praseodymium master alloy to the first aluminum liquid described in S2 for stage-by-stage refining to obtain a third aluminum liquid; S4, degassing and deslagging the third aluminum liquid described in S3 to obtain a fourth aluminum liquid; S5. Continuously casting, induction heating, rolling, annealing and cold drawing the fourth aluminum liquid described in S4 to obtain an aluminum alloy wire.

2. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: The chemical composition and mass percentage of the aluminum alloy material are: Si 0-0.03%, Fe 0-0.06%, Zr 0.5%-0.9%, Er 2.0%-3.0%, Nd 0.5%-1.0%, Pr 0.3%-0.7%, B 0-0.0005%, the sum of Cr, Mn, V and Ti is 0-0.0005%, and the balance is Al and other inevitable impurities.

3. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S1, the melting temperature is 800°C-850°C; And / or, the refining is performed under the conditions of nitrogen and a granular refining agent for 20 min-30 min, and then left to stand for 20 min-30 min.

4. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S2, the stirring is carried out under nitrogen for 10 min to 20 min, and then the mixture is allowed to stand for 10 min to 20 min.

5. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S3, the staged refining includes primary refining and secondary refining; the primary refining is performed under nitrogen and a granular refining agent at 800°C-850°C for 20min-30min, and then allowed to stand for 10min-20min; the secondary refining is performed under argon and a sodium-free refining agent at 800°C-850°C for 20min-30min, and then allowed to stand for 40min-60min.

6. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S5, the process parameters of the continuous casting are: casting temperature is 740℃-770℃, casting speed is 4t / h-5t / h, cooling water temperature of the front zone is 10℃-20℃, cooling water temperature of other zones is 25℃-35℃, and billet outlet temperature is 450℃-500℃.

7. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S5, the temperature of the induction heating is 580°C-630°C.

8. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S5, the rolling process parameters are: nominal diameter of 14.5 mm-15.5 mm, rolling temperature of 580°C-630°C, final rolling temperature of 300°C-400°C, and winding temperature of 250°C-300°C.

9. The method for preparing an aluminum alloy wire according to claim 1, characterized in that: In S5, the annealing is divided into three stages. The first stage is annealing at 320°C-360°C for 10h-30h, the second stage is annealing at 430°C-480°C for 40h-100h, and the third stage is cooling to below 300°C within 3h-10h.

10. An aluminum alloy wire prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Aluminum alloy continuous casting and rolling unit molten aluminum crystallizing wheel quenching control system

    CN105238921A

  • Low-cost 63% IACS high-conductivity duralumin conductor and manufacturing method thereof

    CN105950893A

  • Preparation method of heat-resistant aluminum alloy wire

    CN106636695A

  • High strength heat-resisting aluminium alloy wire and manufacturing method thereof

    CN106887266A

  • High-rare-earth-content high-intensity heat-resistance aluminum alloy conducting wire and preparation method thereof

    CN108220693A