Inorganic single-component adhesive as well as preparation method and application thereof

By adding aromatic hydrocarbon compounds, silane coupling agents and other enhancers to the inorganic water glass adhesive, the composite reinforced inorganic water glass adhesive is prepared, which solves the problem of low strength, poor hygroscopic resistance and poor fluidity in the inorganic sand core. The problem has improved the quality and efficiency of the casting process.

CN118926477APending Publication Date: 2024-11-12BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410994605.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing inorganic sand cores have problems such as low strength, poor hygroscopic resistance and poor fluidity during the casting process, which affects the casting quality and efficiency.

Method used

Modified water glass is prepared by hydrothermal reaction using composite reinforced inorganic water glass adhesives, including matrix and a variety of reinforcement agents, such as aromatic hydrocarbon compounds, silane coupling agents, surfactants, organic acids and organic sodium compounds. These reinforcers are added during the casting process to improve the performance of the adhesive.

Benefits of technology

It significantly improves the curing speed, bonding strength, hygroscopic resistance and fluidity of the inorganic sand core, solves the problem of insufficient performance of traditional inorganic sand core, and improves the quality and efficiency of the casting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926477A_ABST
    Figure CN118926477A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of casting, in particular to an inorganic single-component composite enhanced inorganic water glass adhesive which is fast in curing, high in strength, strong in moisture absorption resistance and good in fluidity and a preparation method and application thereof. The composite enhanced inorganic water glass adhesive is prepared from the following components in parts by mass: 35 to 60 parts of sodium silicate powder, 0.1 to 10 parts of lithium polyacrylate, 0.1 to 15 parts of potassium polymetaphosphate, 35 to 60 parts of deionized water, 0.1 to 20 parts of aromatic hydrocarbon compound and 0.1 to 30 parts of silane coupling agent. The composite enhanced inorganic water glass adhesive is provided by modifying water glass and effectively changing the curing mechanism of the adhesive and further exploring the formula of materials in a matrix of the modified water glass, so that the problems of low strength, poor flowability and poor moisture absorption resistance of inorganic molding sand are effectively solved; meanwhile, as a single-component adhesive, the adhesive disclosed by the invention can be directly used, so that a mixing process required by a double-component adhesive is avoided, and the adhesive has a wide application prospect in the aspect of bonding of molding sand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of casting technology, and in particular to an inorganic single-component composite reinforced inorganic water glass adhesive with fast curing, high strength, strong moisture absorption resistance and good fluidity, and a preparation method and application thereof. Background Art

[0002] As society's urgent demand for energy conservation and emission reduction and new energy vehicles continues to increase, the automotive industry's demand for large-size hollow thin-walled aluminum alloy castings such as aluminum alloy subframes and motor housings has also increased. However, in the traditional sand core preparation process, toxic organic sodium compound binders are often used, which not only releases a large amount of toxic gases and air pollutants, posing a threat to operators and the environment, but is also not conducive to sustainable development.

[0003] In order to solve this problem, it is urgent to find a new environmentally friendly inorganic adhesive material to replace the traditional organic sodium compounds. This not only improves the sustainability of casting binders, but also effectively reduces the harm to human health and the environment. The introduction of new inorganic adhesive materials will provide a more environmentally friendly and healthier option for the production of automotive aluminum alloy castings, and contribute to the sustainable development of the industry. In recent years, inorganic adhesives, especially those with inorganic water glass as the main component, have been widely used in the production of casting sand cores and have become green and environmentally friendly adhesives in the foundry industry. However, there are currently some technical difficulties in the preparation of inorganic sand cores, including low sand core strength, poor moisture absorption resistance, and poor sand core fluidity. Improving the curing speed, strength, fluidity and hygroscopicity of inorganic sand cores is the key to improving casting quality and efficiency. Common improvement methods include optimizing the sand core formula, adjusting the raw material ratio, selecting suitable sand, binders and additives; drying and pre-treating the sand to reduce the moisture content and improve fluidity; using surface treatment agents or lubricants to improve the surface quality of the sand; adjusting the curing conditions to ensure that the sand core is fully cured; adding modifiers or nanomaterials to enhance the performance of the sand core. The comprehensive application of these methods and technologies can effectively improve the performance of inorganic sand cores, improve the quality and efficiency of the casting process, and meet the requirements of different castings. This also prompted the urgent research and development of new inorganic binders to improve the comprehensive performance of sand cores and ensure industrial production efficiency, which has become an important topic in the current research field.

[0004] It should be noted that the information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or suggestion in any form that the information constitutes the prior art known to those skilled in the art. Summary of the invention

[0005] In view of this, the first technical problem to be solved by the present invention is to provide a composite reinforced inorganic water glass adhesive that can simultaneously improve the strength, moisture absorption resistance and fluidity of inorganic sand cores in view of the current status of the above-mentioned prior art.

[0006] The second technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned composite reinforced inorganic water glass adhesive.

[0007] The third technical problem to be solved by the present invention is to provide a method for preparing composite reinforced inorganic water glass adhesive molding sand, that is, a method for applying the composite reinforced inorganic water glass adhesive to inorganic molding sand.

[0008] To achieve the above objectives, this application adopts the following technical solutions:

[0009] In the first aspect, the present application provides a composite reinforced inorganic water glass adhesive, including a matrix and a first reinforcing agent, wherein the matrix includes the following components in parts by mass: 35 to 60 parts of sodium silicate powder, 0.1 to 10 parts of lithium polyacrylate, 0.1 to 15 parts of potassium polymetaphosphate, and 35 to 60 parts of ionized water; the first reinforcing agent includes an aromatic hydrocarbon compound and a silane coupling agent; wherein 0.1 to 20 parts of aromatic hydrocarbon compounds and 0.1 to 30 parts of silane coupling agents are added to 100 parts of the matrix to obtain an adhesive A, and the adhesive A is used as the composite reinforced inorganic water glass adhesive.

[0010] Furthermore, the adhesive is further added with a second reinforcing agent, which includes: a surfactant and a modified silicone oil; wherein, 0.01 to 10 parts of the surfactant are added to 100 parts of the adhesive A to obtain an adhesive B, and the adhesive B is used as the composite reinforced inorganic water glass adhesive.

[0011] Furthermore, the adhesive is further added with a third reinforcing agent, and the third reinforcing agent includes: an organic acid and an organic sodium compound; wherein, 1 to 20 parts of organic acid and 1 to 20 parts of organic sodium compound are added to 100 parts of the adhesive A or the adhesive B to obtain an adhesive C, and the adhesive C is used as the composite reinforced inorganic water glass adhesive.

[0012] In a second aspect, the present application provides a method for preparing the composite reinforced inorganic water glass adhesive of the first aspect, comprising the following steps:

[0013] (1) Preparation of modified water glass matrix: prepare 35-60 parts of sodium silicate powder (main raw material of water glass), 0.1-10 parts of lithium polyacrylate (modifier), 0.1-15 parts of potassium polymetaphosphate (modifier) ​​and 35-60 parts of deionized water (as solvent and reaction medium); put the above sodium silicate powder, lithium polyacrylate, potassium polymetaphosphate and deionized water into a reaction container to ensure that the components are evenly mixed; place the mixture in a hydrothermal reaction equipment, set the reaction temperature to 140-160°C, and the reaction time to 8-12 hours to form modified water glass.

[0014] (2) Adding the first reinforcing agent: adding 0.1 to 20 parts of aromatic hydrocarbon compounds and 0.1 to 30 parts of silane coupling agents to 100 parts of the modified water glass prepared in step (1), mixing them evenly, and obtaining adhesive A, which is used as the composite reinforced inorganic water glass adhesive. In the formula, the aromatic hydrocarbon compound helps to adjust the fluidity of the adhesive and improve the bonding strength of the adhesive, and the silane coupling agent is used to improve the bonding force between the adhesive and the filler.

[0015] Furthermore, the preparation method further comprises the following steps:

[0016] (3) Adding a second reinforcing agent: Add 0.01 to 10 parts of a surfactant to 100 parts of the adhesive A, mix them evenly, and obtain an adhesive B. The adhesive B is used as the composite reinforced inorganic water glass adhesive. The surfactant is dissolved or dispersed in the adhesive by stirring or mixing, which can improve the dispersibility, wettability and stability of the adhesive.

[0017] Furthermore, the preparation method further comprises the following steps:

[0018] (4) On the basis of 100 parts of the adhesive A or the adhesive B, 1 to 20 parts of organic acid and 1 to 20 parts of organic sodium compound are added and mixed uniformly to obtain adhesive C, and the adhesive C is used as a composite reinforced inorganic water glass adhesive. In the formula, the organic acid can improve the hydrolysis resistance and stability of the adhesive, and the addition of the organic sodium compound can enhance the adhesion and wear resistance of the adhesive.

[0019] The present application further provides a method for preparing composite reinforced inorganic water glass adhesive molding sand, comprising the following steps:

[0020] Add raw sand into a sand mixer for sand mixing, add a composite reinforced inorganic water glass adhesive by adding in batches or continuously, ensure that the adhesive fully covers and is evenly mixed with the raw sand particles, and obtain a molding sand mixture; wherein the composite reinforced inorganic water glass adhesive is the composite reinforced inorganic water glass adhesive described in the first aspect above or the composite reinforced inorganic water glass adhesive prepared according to the preparation method described in the second aspect above; wherein, 1 to 10 parts of the composite reinforced inorganic water glass adhesive are added to every 100 parts of raw sand, and the sand mixing time after adding the composite reinforced inorganic water glass adhesive is 1 to 2 minutes.

[0021] The beneficial effects of the present application are as follows: the present application provides a composite reinforced inorganic water glass adhesive for casting, which effectively solves the problems of low strength, poor fluidity and poor moisture absorption resistance of inorganic molding sand, and improves the comprehensive performance of molding sand; at the same time, the adhesive of the present application can be used directly because it is a single-component adhesive, avoiding the mixing process required for a two-component adhesive, improving the user experience, and has broad application prospects in the bonding of molding sand. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0023] Figure 1 This is a test diagram of the bending strength of the inorganic sand block samples prepared in each embodiment and comparative example provided in this application;

[0024] Figure 2 This is a test chart of the anti-hygroscopicity of the inorganic sand block samples prepared in the various embodiments and comparative examples provided in this application;

[0025] Figure 3 This is a test diagram of the bending strength of the inorganic sand block samples prepared in Examples 1, 2 and Comparative Examples 1, 2 provided in this application;

[0026] Figure 4 This is a test chart of the anti-hygroscopicity of the inorganic sand block samples prepared in Examples 1, 2 and Comparative Examples 1, 2 provided in the present application;

[0027] Figure 5 This is a test diagram of the bending strength of the inorganic sand block samples prepared in Examples 3, 4 and Examples 1, 2 provided in this application;

[0028] Figure 6 This is a test chart of the anti-hygroscopicity of the inorganic sand block samples prepared in Examples 3, 4 and Examples 1, 2 provided in this application;

[0029] Figure 7This is a test diagram of the bending strength of the inorganic sand block samples prepared in Examples 5, 6 and Comparative Examples 1, 2 provided in this application;

[0030] Figure 8 This is a test chart of the anti-hygroscopicity of the inorganic sand block samples prepared in Examples 5, 6 and Comparative Examples 1, 2 provided in the present application;

[0031] Fig. 9 This is a test diagram of the bending strength of the inorganic sand block samples prepared in Example 7 and Comparative Examples 1 and 2 provided in this application;

[0032] Fig.10 This is a test diagram of the anti-hygroscopicity of the inorganic sand block samples prepared in Example 7 and Comparative Examples 1 and 2 provided in the present application;

[0033] Fig.11 This is a test diagram of the bending strength of the inorganic sand block samples prepared in Comparative Examples 1, 2 and 3 provided in this application;

[0034] Fig.12 This is a test chart of the anti-hygroscopicity of the inorganic sand block samples prepared in Comparative Examples 1, 2 and 3 provided in this application;

[0035] Fig.13 This is a schematic structural diagram of a curved inorganic sand sample for testing the fluidity of inorganic sand used in each embodiment and comparative example of the present application;

[0036] Fig.14 Schematic diagram of the structure of the inorganic sand block sample used in the sand core bending strength test in each embodiment and comparative example of the present application. DETAILED DESCRIPTION

[0037] The following is a more detailed description of the technical features and advantages of the present application in combination with embodiments and comparative examples, so that the advantages and features of the present application can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present application.

[0038] The embodiment of the present application provides a composite reinforced inorganic water glass adhesive, including a matrix and a first reinforcing agent; wherein the matrix includes the following components in parts by mass: 35-60 parts of sodium silicate powder, 0.1-10 parts of lithium polyacrylate, 0.1-15 parts of potassium polymetaphosphate, and 35-60 parts of deionized water; the first reinforcing agent includes an aromatic hydrocarbon compound and a silane coupling agent; wherein 0.1-20 parts of aromatic hydrocarbon compounds and 0.1-30 parts of silane coupling agents are added to 100 parts of the matrix to obtain adhesive A, and adhesive A is used as the composite reinforced inorganic water glass adhesive. In the adhesive formula of the embodiment of the present application, lithium polyacrylate and potassium polymetaphosphate are introduced into the aqueous solution of sodium silicate, and these two components enhance and adjust the modulus of the sodium silicate solution to form a modified water glass matrix. Unmodified sodium silicate solution has the defects of slow curing speed, low bonding strength, poor anti-hygroscopicity, and poor fluidity of molding sand after adding molding sand. The embodiments of the present application can adjust the parameters such as modulus, cation content, solid content, etc. of sodium silicate by modifying the sodium silicate, thereby improving the curing speed, bonding strength and anti-hygroscopicity of the sodium silicate adhesive to a certain extent. The modified sodium silicate adhesive exhibits more outstanding performance and can have a wider range of applications. And by adding aromatic hydrocarbon compounds and silane coupling agents to the modified water glass matrix, the curing speed, bonding strength and anti-hygroscopicity of the adhesive can be greatly improved.

[0039] In the formula, the aromatic hydrocarbon compound can preferably be one or a mixture of o-bromotrifluoromethoxybenzene, 4,4'-diacetylbiphenyl, 1,3-diacetylbenzene, p-diethoxybenzene, 3,4-diaminotoluene, 2-difluoromethoxybromobenzene, n-dodecylbenzene and 3,5-dihydroxytoluene.

[0040] The silane coupling agent can preferably be one or a mixture of γ-(2,3-epoxypropyl)propyltrimethoxysilane, p-phenylvinyltrimethoxysilane, (3-epoxypropyl)trimethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxysilane and N-vinylbenzyl-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride.

[0041] In some preferred embodiments of the present application, the preparation method of the above-mentioned composite reinforced inorganic water glass adhesive comprises the following steps:

[0042] (1) Preparation of modified water glass matrix: 35-60 parts of sodium silicate powder, 0.1-10 parts of lithium polyacrylate, 0.1-15 parts of potassium polymetaphosphate and 35-60 parts of deionized water are mixed, and modified water glass is obtained by hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 140-160°C, preferably 150°C; the reaction time is 8-12 hours, preferably 10 hours. Hydrothermal reaction is a chemical reaction carried out under high temperature and high pressure conditions, which helps to promote the reaction and combination between raw materials. The use of hydrothermal method to prepare the above-mentioned modified water glass can not only improve the utilization rate of raw materials, but also solve the problem of hydrogen generation caused by silicon in the by-product. It is a safe, stable water glass manufacturing method with high raw material utilization and good product quality.

[0043] (2) Adding a first reinforcing agent: Add 0.1 to 20 parts of an aromatic hydrocarbon compound and 0.1 to 30 parts of a silane coupling agent to 100 parts of the modified water glass prepared in step (1), mix well, and obtain an adhesive A, which is used as the composite reinforced inorganic water glass adhesive.

[0044] Preferably, the above step (1) may specifically include the following steps: adding 0.1 to 10 parts of lithium polyacrylate and 0.1 to 15 parts of potassium polymetaphosphate to 35 to 60 parts of deionized water, stirring until the lithium polyacrylate and potassium polymetaphosphate are dissolved; then adding 0 to 50 parts of sodium silicate powder, stirring until the sodium silicate is dissolved. The stirring rate is 500 to 2000 rpm, preferably 800 rpm; the stirring temperature is room temperature, preferably 25°C. The test results of the applicant show that the above addition order is conducive to the formation of a transparent and stable solution, and is also conducive to the dissolution of lithium polyacrylate and potassium polymetaphosphate.

[0045] In a preferred embodiment of the present application, the formula of the composite reinforced inorganic water glass adhesive can further add a second reinforcing agent on the basis of the above-mentioned adhesive A, and the second reinforcing agent includes a surfactant. Specifically, 0.01 to 10 parts of surfactant are added to 100 parts of the adhesive A prepared in step (2), mixed evenly, and adhesive B is obtained, and adhesive B is used as the composite reinforced inorganic water glass adhesive. In the formula of this embodiment, by adding a surfactant to the matrix of the modified water glass, the surface tension of the water glass liquid and the wetting properties for the molding sand and metal can be changed, and the friction resistance between the gravel and the wall of the sand-shooting mold can be effectively reduced, thereby improving the fluidity of the molding sand mixture. Among them, the surfactant can preferably be an anionic surfactant or a nonionic surfactant. The reason for selecting anionic and nonionic surfactants is that cationic surfactants will react chemically with water glass, resulting in the production of white flocculent insolubles in the water glass, and will cause the water glass adhesive to lose its function, so anionic surfactants and nonionic surfactants that do not react with water glass are selected.

[0046] Further preferably, the above-mentioned surfactant can be an anionic surfactant, and more preferably one or a mixture of potassium larate, sodium 4-((3-((2,4-dimethylphenyl)azo)-2,4-dihydroxyphenyl)azo)benzenesulfonate, disteardimethylammonium hectorite, trioleylglycerol methylaminoethyl sulfonic acid and basic tall oil fatty acid manganese salt.

[0047] In a more preferred embodiment of the present application, the formula of the composite reinforced inorganic water glass adhesive can further add a third reinforcing agent on the basis of adhesive A or adhesive B, and the third reinforcing agent includes an organic acid and an organic sodium compound; specifically, 1 to 20 parts of organic acid and 1 to 20 parts of organic sodium compound are added to 100 parts of adhesive A or 100 parts of adhesive B, and mixed evenly to obtain adhesive C, and adhesive C is used as the composite reinforced inorganic water glass adhesive. In the formula of this embodiment, the added organic acid can form a high-functionality cross-linking site between water glass and sand particles, thereby improving the strength of molding sand.

[0048] Preferably, the organic acid may be one or a mixture of oxalic acid, succinic acid, polyaspartic acid, polyacrylic acid and benzoic acid copolymer.

[0049] The added organic sodium compound is preferably a mixture of one or more of sodium gluconate, sodium methoxide, sodium acetate, sodium tartrate and sodium ethoxide. The reason for selecting the organic sodium compound is that it can improve the bonding performance of the water glass adhesive while improving the stability of the sand core and extending the shelf life.

[0050] In summary, the component scheme of the composite reinforced inorganic water glass adhesive in the embodiment of the present application can be selected from the following schemes:

[0051] (1) Modified water glass matrix + aromatic hydrocarbon compound, silane coupling agent;

[0052] (2) modified water glass matrix + aromatic hydrocarbon compound, silane coupling agent + surfactant;

[0053] (3) modified water glass matrix + aromatic hydrocarbon compound, silane coupling agent + organic acid, organic sodium compound;

[0054] (4) Modified water glass matrix + aromatic hydrocarbon compound, silane coupling agent + surfactant + organic acid, organic sodium compound. When preparing the composite reinforced inorganic water glass adhesive, the order of adding the components can be adjusted as needed.

[0055] The composite reinforced inorganic water glass adhesive provided in the embodiment of the present application is used for casting inorganic sand, which can take into account the strength, fluidity and moisture absorption resistance of the molding sand, thereby effectively improving the comprehensive performance of the inorganic sand core.

[0056] The present application further provides a storage method for the composite reinforced inorganic water glass adhesive, comprising the following steps:

[0057] 1. Choose a suitable storage container: Choose a clean, dry, well-sealed container, such as a plastic bucket, glass bottle or metal container. Make sure the surface of the container is clean and free of residue.

[0058] 2. Clearly label: Mark the container with important information such as the name, batch number, production date and expiration date of the adhesive. This helps track and manage the use of the adhesive.

[0059] 3. Avoid direct sunlight: Place the storage container in a cool, dry place, away from direct sunlight and heat sources. Avoid long-term exposure to high temperature to prevent affecting the quality of the adhesive.

[0060] 4. Regular inspection and maintenance: Regularly check the sealing and appearance of the storage container to ensure that there is no damage or leakage. If any problems are found, replace the container or repair the seal in time.

[0061] 5. Avoid cross contamination: Store different types or batches of adhesives separately to avoid cross contamination and chemical reactions, and ensure the stability and performance of each adhesive.

[0062] 6. Strictly control humidity: Maintain a dry environment in the storage area. You can use a dehumidifier or a hygrometer to monitor the humidity level to prevent the adhesive from absorbing moisture and causing performance degradation.

[0063] 7. Proper disposal of waste: When handling adhesive packaging and waste, they should be classified and properly handled in accordance with local environmental regulations to avoid pollution to the environment.

[0064] The above steps help to ensure the quality and stability of the composite reinforced inorganic water glass adhesive, extend its service life, and ensure that it can be used safely and effectively when needed.

[0065] In the embodiment of the present application, the method for preparing an inorganic molding sand mixture using the above-mentioned composite reinforced inorganic water glass adhesive specifically comprises the following steps:

[0066] 1. Prepare sand mixing equipment: Prepare the sand mixer or other suitable mixing equipment and ensure that the equipment is clean and free of impurities.

[0067] 2. Add raw sand: put the raw sand to be processed into the sand mixing equipment.

[0068] 3. Adding composite reinforced inorganic adhesive: gradually add the required amount of composite reinforced inorganic water glass adhesive to the raw sand. It can be added in batches or continuously to ensure that the adhesive is fully covered and evenly mixed with the raw sand particles. The addition amount is 1 to 10 parts of composite reinforced inorganic water glass adhesive per 100 parts by mass of raw sand.

[0069] 4. Control the mixing time: When adding adhesive, control the mixing time to ensure uniform mixing without over-curing or loss of adhesive activity. The recommended mixing time is usually between 1 and 2 minutes.

[0070] 5. Observe the mixing effect: By observing the particle state and color changes of the molding sand inside the sand mixing equipment, determine whether the mixing has reached the ideal state.

[0071] 6. Storage and use: Store the mixed inorganic sand in a dry, clean and sealed container to avoid moisture and impurity contamination for subsequent casting process.

[0072] By executing the above steps, inorganic molding sand with stable quality and superior performance can be obtained. The obtained molding sand mixture has good fluidity and high strength, is suitable for various casting processes, and improves the quality and production efficiency of castings.

[0073] In the examples / comparative examples of the present application, in order to verify the performance indicators such as fluidity, strength and anti-hygroscopicity of the molding sand mixture, the prepared molding sand mixture is added to a new hot air-warm core box composite hardening process sample machine, and molded by hot air heating to obtain molding sand block samples. The number of molding sand block samples obtained and the degree of mold filling are used as standards for testing the fluidity of the molding sand mixture, and the flexural strength of the molding sand block samples after being placed at room temperature for different periods of time and the flexural strength after being placed at room temperature and high humidity for different periods of time are measured. Among them, the shapes of the molding sand block samples used are curved and strip-shaped, which are convenient for testing fluidity and testing in a bending test machine, respectively. Please refer to Fig.13 , which is a schematic diagram of the structure of a curved sand block specimen; please refer to Fig.14 , which is a schematic diagram of the structure of the strip molding sand block sample.

[0074] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0075] The raw materials and reagents used in the following examples and comparative examples are all commercially available or homemade.

[0076] Comparative Example 1

[0077] Add 0.2g of lithium polyacrylate and 0.2g of potassium polymetaphosphate to 50g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 50g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 100.4g of modified water glass adhesive.

[0078] Comparative Example 2

[0079] Add 10g of lithium polyacrylate and 15g of potassium polymetaphosphate to 50g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 60g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 135g of modified water glass adhesive.

[0080] Comparative Example 3

[0081] Add 40g of sodium silicate to 60ml of water and stir until the sodium silicate is dissolved to obtain a mixture. The mixing temperature of the above mixing process is 25°C and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor and perform a hydrothermal reaction at 150°C for 10h to obtain 100g of water glass adhesive.

[0082] Example 1

[0083] 1) Preparation of modified water glass:

[0084] Add 2g of lithium polyacrylate and 2g of potassium polymetaphosphate to 50g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 50g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 104g of modified water glass adhesive.

[0085] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0086] 1 g of 3,5-dihydroxytoluene and 2 g of (3-glycidoxypropyl)trimethoxysilane were added to 100 g of the modified water glass obtained in step 1) to obtain 103 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0087] Example 2

[0088] 1) Preparation of modified water glass:

[0089] Add 0.2g of lithium polyacrylate and 0.2g of potassium polymetaphosphate to 60g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 60g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 120.4g of modified water glass adhesive.

[0090] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0091] 5 g of 3,5-dihydroxytoluene and 5 g of (3-glycidoxypropyl)trimethoxysilane were added to 100 g of the modified water glass obtained in step 1) to obtain 110 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0092] Example 3

[0093] 1) Preparation of modified water glass:

[0094] Add 1g of lithium polyacrylate and 1g of potassium polymetaphosphate to 70% water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 70g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10 hours to obtain 142g of modified water glass adhesive.

[0095] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0096] 100 g of the modified water glass prepared in step 1) was added with 1 g of 3,5-dihydroxytoluene and 2 g of (3-glycidoxypropyl) trimethoxysilane, and then 0.4 g of trioleylglycerol methylaminoethylsulfonic acid and 2 g of epoxy-modified silicone oil were added after stirring to obtain 105.4 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0097] Example 4

[0098] 1) Preparation of modified water glass:

[0099] Add 1g of lithium polyacrylate and 1g of potassium polymetaphosphate to 60g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 40g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 102g of modified water glass adhesive.

[0100] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0101] 1 g of 1,3-diacetylbenzene and 2 g of p-styryltrimethoxysilane were added to 100 g of the modified water glass obtained in step 1), and then 1 g of trioleylglycerol methylaminoethylsulfonic acid was added after stirring to obtain 104 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0102] Example 5

[0103] 1) Preparation of modified water glass:

[0104] Add 0.2g of lithium polyacrylate and 0.2g of potassium polymetaphosphate to 50g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 50g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 100.4g of modified water glass adhesive.

[0105] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0106] 2 g of p-diethoxybenzene and 4 g of (3-glycidoxypropyl)trimethoxysilane were added to 100 g of the modified water glass obtained in step 1), and then 1 g of sodium N,N-dicarboxylic acid amino-2-hydroxypropane sulfonate and 2 g of sodium ethoxide were added after stirring to obtain 106 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0107] Example 6

[0108] 1) Preparation of modified water glass:

[0109] Add 5g of lithium polyacrylate and 2g of potassium polymetaphosphate to 50g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 50g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution into a hydrothermal reactor, and perform hydrothermal reaction at 150°C for 10h to obtain 107g of modified water glass adhesive.

[0110] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0111] 2 g of 3,5-dihydroxytoluene and 3 g of N-2-aminoethyl-3-aminopropyltriethoxysilane were added to 100 g of the modified water glass obtained in step 1), and then 8 g of succinic acid and 4 g of sodium ethoxide were added after stirring to obtain 117 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0112] Example 7

[0113] 1) Preparation of modified water glass:

[0114] Add 1g of lithium polyacrylate and 2g of potassium polymetaphosphate to 55g of water, stir until lithium polyacrylate and potassium polymetaphosphate are completely dissolved; then add 45g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixture. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and perform a hydrothermal reaction at 150°C for 10h to obtain 103g of modified water glass adhesive.

[0115] 2) Preparation of composite reinforced inorganic water glass adhesive:

[0116] 100 g of the modified water glass prepared in step 1) was added with 1 g of 3,5-dihydroxytoluene and 2 g of (3-glycidoxypropyl) trimethoxysilane, and then 0.4 g of trioleylglycerol methylaminoethylsulfonic acid was added after stirring, and then 3 g of polyaspartic acid and 2 g of sodium ethoxide were added after stirring to obtain 108.4 g of a composite reinforced inorganic modified water glass adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0117] The inorganic molding sand mixture is further prepared by using the adhesive prepared in each embodiment and comparative example, and then the molding sand block sample is obtained by combining with the preparation process of the inorganic sand core, and the performance test of the obtained molding sand block sample is carried out to examine the performance of the corresponding adhesive. The specific method is as follows:

[0118] Weigh 2.5 kg of 50 / 100 mesh Dalin scrubbing sand and put it into a sand mixer, weigh 100 g of the inorganic modified water glass adhesive prepared in Example 1, add the mixed inorganic modified water glass adhesive to the scrubbing sand while mixing the sand, and mix the sand for 1 minute to obtain a molding sand mixture. Put the mixed molding sand mixture into a hot air-warm core box composite hardening process sample machine, use room temperature air to blow the molding sand mixture from the sand storage tank into the mold, the sand shooting time is 2 seconds, and then under the condition of a mold temperature of 180°C, continue to pass hot air into the mold for 40 seconds (hot air temperature 120°C, pressure 4 bar), so that the inorganic sand mixture is solidified to obtain the following Fig.14 The strip molding sand block specimen shown and Fig.13 The curved molding sand block specimen is shown.

[0119] The above steps were repeated to prepare corresponding molding sand mixtures using the inorganic adhesives of Examples 2 to 7 and Comparative Examples 1 to 3, and then strip molding sand block samples and curved molding sand block samples were further prepared.

[0120] The obtained strip-shaped molding sand block samples were subjected to flexural strength tests and moisture absorption resistance tests, and the curved molding sand block samples were tested for fluidity.

[0121] Specifically, the bending strength of the strip inorganic sand block specimens was tested at 30 seconds and at 25° C., 20% RH humidity environment for 1 hour and 24 hours.

[0122] Specifically, the bending strength of the strip inorganic sand block samples was tested at 25° C. and 60% RH humidity environment for 1 day, 3 days, 5 days and 7 days. The higher the bending strength, the better the moisture absorption resistance.

[0123] Specifically, the curved inorganic sand block sample is used to test the fluidity of the inorganic sand mixture. If the fluidity of the inorganic sand mixture is not good, it will not be able to fill the entire curved mold. At the same time, if the fluidity of the inorganic sand mixture is not good, the air will make a hole in the middle of the curved inorganic sand block sample, and the inorganic sand next to it cannot fall, and the compactness of the inorganic sand in the curved inorganic sand block sample is also low. Therefore, the higher the degree of filling of the curved mold and the higher the compactness of the inorganic sand in the curved inorganic sand block sample, the better the fluidity of the inorganic sand mixture. In the embodiment of the present application, the standard for assessing the fluidity of the inorganic sand mixture is that if the inorganic sand mixture fills the curved mold, it is a qualified sample, and if it is not filled, it is an unqualified sample. The qualified rate is calculated. The higher the qualified rate, the higher the single root quality of the qualified sample and the more the total number of roots, the better the fluidity of the inorganic sand mixture.

[0124] Among them, the new hot air-warm core box composite hardening process sample machine is an inorganic sample machine sold by Suzhou Ailid Intelligent Equipment Co., Ltd., model IWJ01. The scrubbing sand used is a special foundry sand with certain particle size, dust content and humidity requirements. The scrubbing sand can also be replaced by sand that meets the casting standards.

[0125] The fluidity test results of the inorganic sand mixtures prepared in the embodiments and comparative examples are shown in Table 1, and the bending strength test results are shown in Table 2. Figure 1 The test results of its anti-hygroscopicity are shown in Figure 2 shown.

[0126] Table 1 Fluidity test results of various embodiments / comparative examples

[0127]

[0128] As shown in Table 1, the difference between Examples 1 and 2 and Comparative Examples 1 and 2 is that aromatic hydrocarbon compounds and silane coupling agents are added. The experimental results show that after adding aromatic hydrocarbon compounds and silane coupling agents, the number and qualified rate of the prepared qualified curved samples are slightly improved. This shows that the addition of aromatic hydrocarbon compounds and silane coupling agents can slightly improve the fluidity of inorganic sand.

[0129] As shown in Table 1, the difference between Examples 3 and 4 and Examples 1 and 2 is that a surfactant is added. The experimental results show that after adding the surfactant and modified silicone oil, the number and qualified rate of the prepared qualified curved samples are significantly improved. This shows that the addition of surfactants and modified silicone oil can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the sand injection amount of the instrument, which is of great significance for the realization of mechanized sand injection.

[0130] As shown in Table 1, the difference between Examples 5 and 6 and Comparative Examples 1 and 2 is that organic acid and organic sodium compound are added. The experimental results show that after adding organic acid and organic sodium compound, the number and qualified rate of the prepared qualified curved samples are slightly improved. This shows that the addition of organic acid and organic sodium compound can slightly improve the fluidity of inorganic sand.

[0131] As shown in Table 1, the difference between Example 7 and Examples 5 and 6 is that a surfactant is added. The experimental results show that after adding the surfactant and modified silicone oil, the number and qualified rate of the prepared qualified curved samples are significantly improved. This shows that the addition of surfactants and modified silicone oil can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the sand injection amount of the instrument, which is of great significance for the realization of mechanized sand injection.

[0132] like Figure 3 , Figure 4 As shown, the difference between Examples 1 and 2 and Comparative Examples 1 and 2 is that aromatic hydrocarbon compounds and silane coupling agents are added. The experimental results show that the addition of aromatic hydrocarbon compounds and silane coupling agents significantly improves the 30s hot strength, 1h and 24h cold strength and residual strength of the sand core after 7 days of storage. It shows that the addition of aromatic hydrocarbon compounds and silane coupling agents can greatly improve the curing speed, bonding strength and moisture absorption resistance of inorganic sand.

[0133] like Figure 5 , Figure 6 As shown, the difference between Examples 3 and 4 and Examples 1 and 2 is the addition of surfactants. The experimental results show that the addition of surfactants and modified silicone oils can keep the 30s hot strength, 1h and 24h cold strength and 7-day storage residual strength of the sand core almost unchanged. This shows that the addition of multiple surfactants and modified silicone oils can greatly improve the fluidity of inorganic sand while having almost no effect on the curing speed, bonding strength and moisture absorption resistance.

[0134] like Figure 7 , Figure 8 As shown, the difference between Examples 5 and 6 and Comparative Examples 1 and 2 is that organic acid and organic sodium compound are added. The experimental results show that the addition of organic acid and organic sodium compound significantly improves the 30s hot strength, 1h and 24h cold strength and 7-day storage residual strength of the sand core. It shows that the addition of organic acid and organic sodium compound can greatly improve the curing speed, bonding strength and moisture absorption resistance of inorganic sand.

[0135] like Fig. 9 , Fig.10 As shown, compared with Comparative Examples 1 and 2, Example 7 differs in that an aromatic hydrocarbon compound, a silane coupling agent, a surfactant, an organic acid and an organic sodium compound are added. The experimental results show that the addition of aromatic hydrocarbon compounds, silane coupling agents, organic acids and organic sodium compounds significantly improves the 30s hot strength, 1h and 24h cold strength and residual strength of the sand core after 7 days of storage. This shows that the synergistic effect of aromatic hydrocarbon compounds, silane coupling agents, organic acids and organic sodium compounds can greatly improve the curing speed, bonding strength and moisture absorption resistance of inorganic sand.

[0136] like Fig.11 , Fig.12 As shown, the difference between Comparative Examples 1 and 2 and Comparative Example 3 is that a modified water glass adhesive is used. The experimental results show that the use of the modified water glass adhesive improves the 30s hot strength, 1h and 24h cold strength and 7-day storage residual strength of the sand core. This shows that the modified water glass formula of the present invention can greatly improve the curing speed, bonding strength and moisture absorption resistance of inorganic sand.

[0137] It should be noted that in Examples 1 to 7, the same weight of components is used to prepare the modified water glass of step 1), which is to facilitate the performance comparison with the comparative example and other embodiments. In other embodiments of the present application, the applicant uses other weight ratios of each component to prepare a composite reinforced inorganic water glass adhesive, and similar test results are obtained. Specifically, the basic formula of the composite reinforced inorganic water glass adhesive includes: 35 to 60 parts of sodium silicate powder, 0.1 to 10 parts of lithium polyacrylate, 0.1 to 15 parts of potassium polymetaphosphate, 35 to 60 parts of deionized water, 0.1 to 20 parts of aromatic hydrocarbon compounds, and 0.1 to 30 parts of silane coupling agents. The preferred formula is to further include: 0.01 to 10 parts of surfactants on the basis of the basic formula. Other preferred formulas are to further include: 1 to 20 parts of organic acids and 1 to 20 parts of organic sodium compounds on the basis of the basic formula or the above preferred formula. The components and contents of the above formulas have been verified by the applicant through a large number of performance test experiments.

[0138] In summary, the composite strong inorganic single-component adhesive provided in the present application can greatly improve the curing speed, strength, moisture absorption resistance and fluidity of the inorganic sand mixture, has broad application prospects in the field of inorganic sand, and is of great significance for realizing mechanized sand injection production.

[0139] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A composite reinforced inorganic water glass adhesive, characterized in that: The invention comprises a matrix and a first reinforcing agent, wherein the matrix comprises the following components in parts by mass: 35 to 60 parts of sodium silicate powder, 0.1 to 10 parts of lithium polyacrylate, 0.1 to 15 parts of potassium polymetaphosphate, and 35 to 60 parts of deionized water; the first reinforcing agent comprises an aromatic hydrocarbon compound and a silane coupling agent; wherein 0.1 to 20 parts of the aromatic hydrocarbon compound and 0.1 to 30 parts of the silane coupling agent are added to 100 parts of the matrix to obtain an adhesive A, and the adhesive A is used as the composite reinforced inorganic water glass adhesive.

2. The composite reinforced inorganic water glass adhesive according to claim 1, characterized in that: The adhesive is further added with a second reinforcing agent, which includes: a surfactant and modified silicone oil; wherein, 0.01 to 10 parts of the surfactant are added to 100 parts of the adhesive A to obtain an adhesive B, and the adhesive B is used as the composite reinforced inorganic water glass adhesive.

3. The composite reinforced inorganic water glass adhesive according to claim 1 or 2, characterized in that: The adhesive is further added with a third reinforcing agent, which includes: an organic acid and an organic sodium compound; wherein, 1 to 20 parts of organic acid and 1 to 20 parts of organic sodium compound are added to 100 parts of the adhesive A or the adhesive B to obtain an adhesive C, and the adhesive C is used as the composite reinforced inorganic water glass adhesive.

4. The preparation method of the composite reinforced inorganic water glass adhesive according to claim 1, wherein The following steps are involved: (1) preparing a modified water glass matrix: mixing 35-60 parts of sodium silicate powder, 0.1-10 parts of lithium polyacrylate, 0.1-15 parts of potassium polymetaphosphate and 5-70 parts of deionized water, and subjecting the mixture to a hydrothermal reaction to obtain the modified water glass; (2) Adding a first reinforcing agent: adding 0.1 to 20 parts of an aromatic hydrocarbon compound and 0.1 to 30 parts of a silane coupling agent to 100 parts of the modified water glass prepared in step (1), mixing them uniformly, and obtaining an adhesive A, which is used as the composite reinforced inorganic water glass adhesive.

5. The preparation method according to claim 4, characterized in that In step (1), the reaction temperature of the hydrothermal reaction is 140-160° C., and the reaction time is 8-12 h.

6. The preparation method according to claim 4, characterized in that The step (1) specifically comprises: adding 0.1 to 10 parts of lithium polyacrylate and 0.1 to 15 parts of potassium polymetaphosphate to 5 to 70 parts of water, stirring until the lithium polyacrylate and potassium polymetaphosphate are dissolved, and then adding 5 to 70 parts of sodium silicate, reacting until the sodium silicate is dissolved.

7. The preparation method according to claim 4, characterized in that The preparation method further comprises: (3) Adding a second reinforcing agent: adding 0.01 to 10 parts of a surfactant to 100 parts of the adhesive A prepared in step (2), mixing them evenly, to obtain an adhesive B, which is used as the composite reinforced inorganic water glass adhesive.

8. The preparation method according to claim 4 or 7, characterized in that The preparation method further comprises: (4) Adding a third reinforcing agent: adding 1 to 20 parts of an organic acid and 1 to 20 parts of an organic sodium compound to 100 parts of the adhesive A prepared in step (2) or the adhesive B prepared in step (3), and mixing them uniformly to obtain an adhesive C, which is used as a composite reinforced inorganic water glass adhesive.

9. A method for preparing composite reinforced inorganic water glass adhesive molding sand, characterized in that: The following steps are involved: Raw sand is added to a sand mixer for sand mixing, and a composite reinforced inorganic water glass adhesive is added by batch addition or continuous addition to ensure that the composite reinforced inorganic water glass adhesive is fully covered and uniformly mixed with the raw sand particles to obtain molding sand; wherein the composite reinforced inorganic water glass adhesive is the composite reinforced inorganic water glass adhesive according to any one of claims 1 to 3 or the composite reinforced inorganic water glass adhesive prepared by the preparation method according to any one of claims 4 to 8; wherein 1 to 10 parts of the composite reinforced inorganic water glass adhesive are added to every 100 parts of raw sand, and the sand mixing time after the addition of the composite reinforced inorganic water glass adhesive is 1 to 2 minutes.