Nano-porous copper heat dissipation material based on composite copper mesh and surface modification combination and preparation method of nano-porous copper heat dissipation material

By pressing a multi-layer copper mesh on the porous copper material and performing hydrophilic surface modification, the problem of insufficient heat dissipation performance of electronic equipment is solved, and efficient boiling heat exchange performance and cost reduction are achieved.

CN118926519APending Publication Date: 2024-11-12NORTH CHINA ELECTRIC POWER UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410998299.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is not effective in improving the heat dissipation performance of electronic devices, especially in miniaturized devices, where common heat dissipation methods are difficult to meet the needs of efficient heat dissipation.

Method used

By pressing a multi-layer copper mesh on the porous copper material and performing hydrophilic surface modification, the bubble disengagement rate and boiling heat exchange coefficient are improved, thereby increasing the peak heat flow density of the convective heat exchange coefficient and improving the heat exchange efficiency.

Benefits of technology

The boiling heat exchange performance is significantly improved. The hydrophobic surface modification shows superior heat exchange performance in the early stage, while the hydrophilic surface modification performs better in the later stage. The combination of the two reduces production costs and improves heat dissipation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926519A_ABST
    Figure CN118926519A_ABST
Patent Text Reader

Abstract

The invention relates to a nano-porous copper heat dissipation material based on combination of a composite copper mesh and surface modification and a preparation method thereof, and the preparation method comprises the following steps: putting a copper salt mixture into a stainless steel mold, and firstly, manually compacting to form a loose structure; sequentially laying a plurality of layers of copper nets with different mesh numbers on the loose structure from top to bottom according to the mesh number from small to large to form a composite gradient copper net, and performing compression molding to obtain a pressed sheet; and sequentially carrying out vacuum sintering, cleaning and drying on the pressed sheet, sequentially carrying out hydrophilic surface modification and hydrophobic surface modification on the improved powder molded porous copper heat dissipation material based on the surface composite copper mesh by adopting a chemical etching method, and finally cleaning and drying to obtain the heat dissipation material. The preparation method is simple, raw materials are low in price, and the production cost can be reduced; the bubble separation rate and the boiling heat transfer coefficient can be improved by pressing multiple layers of copper nets on the surface of the porous copper and conducting hydrophilic and hydrophobic modification on the surface, the corresponding heat flow density value when the convective heat transfer coefficient reaches the peak value is increased, and therefore the heat exchange efficiency is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano material synthesis methods, and specifically relates to a nano porous copper heat dissipation material based on a composite copper mesh and surface modification and a preparation method thereof. Background Art

[0002] At present, electronic devices are showing a trend of compactness and high power, which brings severe challenges to the heat dissipation of electronic devices. Researchers have made many attempts to manage the thermal management of electronic devices, such as common air cooling, water cooling and other heat dissipation methods, but the development trend of miniaturization has limited the use of common convection equipment, and the development of efficient heat dissipation methods is urgent. Surface modification introduces micro-nano structures on the heating surface, increases nucleation sites, improves heat transfer area, changes surface wettability, promotes the generation, growth and detachment of bubbles, and thus significantly improves the heat transfer efficiency of boiling heat exchange.

[0003] Bertossi et al. developed a wettability switchable heating surface by coating a thermosensitive polymer on a stainless steel surface. When the temperature of the heating surface reaches the polymer switching temperature slightly higher than the saturation temperature of the working fluid, the wettability of the polymer changes from hydrophilic to hydrophobic, thereby promoting the nucleation of steam bubbles. During the bubble growth process, the heat conducted near the three-phase contact line causes a local decrease in the polymer temperature, thereby changing the wettability from hydrophobic to hydrophilic. However, the enhancement of boiling HTC is limited to a moderate increase of nearly 20%. Chang et al. found the optimal size and spacing of the surface hydrophobic grid, with the aim of achieving maximum bubble cohesion behavior and rewetting. Deng et al. used a thermal oxidation process to form a nanostructure with superhydrophilic properties on the surface of sintered copper particles, and prepared a spherical copper powder porous structure with a thickness of 0.6 mm and different diameters. The research results showed that the sintered copper powder porous structure enhanced the boiling heat transfer performance, with the maximum HTC and CHF values ​​increased by 151% and 160% of the ordinary copper surface, respectively. At present, the research on surface modification and porous structure design in enhancing boiling heat transfer is independently studying the degree of performance improvement, but the enhancement effect is still poor. Summary of the invention

[0004] The purpose of the present invention is to provide a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification and a preparation method thereof. The preparation method is simple, the raw materials are inexpensive, and the production cost can be reduced. The bubble detachment rate and boiling heat transfer coefficient can be increased by pressing multiple layers of copper mesh on the porous copper surface and performing hydrophilic and hydrophobic modification on the surface, thereby increasing the heat flux density value corresponding to the peak value of the convective heat transfer coefficient, thereby enhancing the heat exchange efficiency.

[0005] To achieve the above object, the present invention is implemented by the following technical solutions:

[0006] A method for preparing a nanoporous copper heat dissipation material based on a composite copper mesh and surface modification, comprising the following steps:

[0007] (1) placing a certain mass of a copper salt mixture into a stainless steel mold, first manually compacting it to form a loose structure, then laying multiple layers of copper meshes of different meshes in order from small to large and from top to bottom on the loose structure to form a composite gradient copper mesh, and pressing and molding to obtain a pressed sheet; the copper salt mixture is prepared by mixing sodium chloride particles and electrolytic copper powder;

[0008] (2) vacuum sintering, cleaning, and drying the pressed tablet obtained in step (1) in sequence to obtain an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh;

[0009] (3) The improved powder-molded porous copper heat dissipation material based on the surface composite copper mesh prepared in step (2) is subjected to hydrophilic surface modification and hydrophobic surface modification in sequence by chemical etching, and finally cleaned and dried to obtain a nanoporous copper heat dissipation material based on the composite copper mesh and surface modification.

[0010] Preferably, in step (1), the multiple layers of copper meshes with different mesh sizes are a layer of 60-mesh copper mesh and a layer of 80-mesh copper mesh.

[0011] Furthermore, in step (3), the hydrophilic surface modification process is:

[0012] a. Preparation of a hydrophilic modification solution: sodium hydroxide was added to deionized water to prepare a sodium hydroxide solution with a concentration of 0.1 g / mL, and potassium persulfate was added to the sodium hydroxide solution, and stirred until the solution was uniformly mixed to obtain a hydrophilic modification solution; the concentration of potassium persulfate in the solution was 13.5 g / L;

[0013] b. The improved powder-molded porous copper heat dissipation material based on the surface composite copper mesh prepared in step (2) is immersed in a hydrophilic modification solution, and then heated in a water bath at 60-80°C for 60-80 minutes. When the surface of the composite copper mesh changes from the original brick red to black, it indicates that the hydrophilic modification is completed.

[0014] Furthermore, in step (3), the hydrophobic surface modification process is: immersing the material after the hydrophilic surface modification in a 0.1 mol / L stearic acid ethanol solution and letting it stand for 4-5 hours.

[0015] Furthermore, in step (3), the cleaning and drying process is as follows: after taking out the material from the stearic acid ethanol solution, ultrasonic cleaning is performed with deionized water and anhydrous ethanol in sequence. After cleaning, the material is placed in a drying oven at 50°C for drying.

[0016] Preferably, in step (2), the pressed tablet is placed in a tubular furnace for vacuum sintering, the heating rate is 8-12°C / min, and the sintering temperature is 650-850°C.

[0017] Preferably, in step (1), the sodium chloride particles are sieved through an 80-mesh sieve; the sodium chloride particles are dried in a vacuum drying oven at 50° C.; the particle size of the electrolytic copper powder is 5 μm; and the mass ratio of the dried sodium chloride particles to the electrolytic copper powder is 1:(4-5).

[0018] Furthermore, in step (1), the preparation process of the copper salt mixture is as follows: drying the sodium chloride particles and placing them together with the electrolytic copper powder into a grinding jar, and then placing the grinding jar in a planetary ball mill for thorough mixing; the ball milling time is 25-35 minutes, and the rotation speed is 150-180rpm; and the tablet press is pressed to obtain a tablet, the tablet press is set to a pressure of 240-280MPa, and the pressure holding time is 180-200s.

[0019] Furthermore, in step (1), the pretreatment process of the copper mesh is: cutting the copper mesh into copper mesh discs according to the specification requirements, then ultrasonically cleaning the copper mesh discs with anhydrous ethanol to remove oil stains, then removing oxides with hydrochloric acid at a concentration of 0.1 mol / L, and then rinsing the copper mesh discs with deionized water and vacuum drying them.

[0020] To achieve the above object, the present invention also provides a method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification obtained by the above preparation method.

[0021] The water surface formation mechanism of the present invention is as follows:

[0022] 1) Hydrophilic surface formation mechanism

[0023] The following chemical reactions mainly occur during the alkaline oxidation process:

[0024] Cu+K 2 S 2 O 8 +2NaOH→Cu(OH) 2 +Na 2 SO 4 +K 2 SO 4 (Ⅰ)

[0025] Cu(OH) 2 →CuO+H 2 O (Ⅱ)

[0026] It can be seen from formula I and formula II that during the alkaline oxidation treatment, a chemical reaction occurs on the surface of the porous copper to generate a hydrophilic group -OH. The hydrophilic group -OH can form hydrogen bonds with water molecules, thereby enhancing the adsorption capacity of porous copper to water. In addition, according to the SEM image, the alkaline oxidation treatment changes the microscopic morphology of the porous copper surface, making it rougher. According to the Wenzel equation, this helps to improve the surface hydrophilicity of the porous copper.

[0027] 2) Hydrophobic surface formation mechanism

[0028] After the alkaline oxidized sample is soaked in stearic acid, the reaction mechanism is as follows:

[0029] Cu(OH) 2 +2CH 3 (CH 2 ) 16 COOH→Cu(CH 3 (CH 2 ) 16 COO 2 +2H 2 O (Ⅲ)

[0030] CuO+2CH 3 (CH 2 ) 16 COOH→Cu(CH 3 (CH 2 ) 16 COO 2 +H 2 O (Ⅳ)

[0031] The principle of hydrophobic modification is mainly achieved by reducing the surface energy of the material surface and increasing the surface roughness. As can be seen from formula III and IV, by grafting low surface energy substances of stearic acid, the hydrophilic group -OH on the surface of porous copper is covered, thereby reducing the adsorption capacity of porous copper surface to water. At the same time, the grafted stearic acid molecular chain is longer, forming a hydrophobic barrier to prevent water molecules from directly contacting the porous copper surface. In addition, it can be seen from the SEM image that a rough microstructure is generated on the hydrophobic porous copper surface. Therefore, when water droplets come into contact with the surface, due to the combined effect of low surface energy and surface roughness, it is difficult for water droplets to spread on the porous copper surface, thereby forming a larger contact angle and a smaller rolling angle, showing hydrophobicity.

[0032] The present invention firstly presses copper meshes of different mesh sizes onto powder-formed porous copper sheets with the best heat transfer performance, and then performs hydrophilic and hydrophobic treatment on the composite copper mesh porous copper. After surface modification, the boiling heat transfer performance of all samples is improved. In the early stage of boiling, the hydrophobic surface shows better heat transfer performance, which is gradually surpassed by the hydrophilic surface in the middle and late stages of boiling. -2 When the hydrophobic surface powder-molded porous copper has a heat transfer coefficient of about 1.8 times that of the unmodified surface, reaching 76000 W·m -2 ·K -1 Although surface modification significantly enhances the boiling heat transfer performance of powder-formed porous copper, the generation of a large number of bubbles hinders the flow of liquid between microstructures, affecting the timely replenishment of fresh liquid to the micro-liquid layer. Therefore, in comparison, the hydrophilic and hydrophobic modification has a smaller improvement on the enhanced heat transfer effect of surface composite copper mesh powder-formed porous copper. At a heat flux density of 180,000 W·m -2 When the heat transfer coefficient of the hydrophobic surface composite copper mesh powder formed porous copper is 1.3 times that of the unmodified surface, which is 82909 W·m -2 ·K -1 Through bubble visualization analysis, under the same heat flux density, the surface modified samples produced more bubbles. The bubbles produced on the hydrophilic surface had a smaller diameter, and the merging phenomenon between bubbles was not obvious; while the bubbles on the hydrophobic surface had a larger diameter before detachment, and some bubbles merged.

[0033] Compared with the prior art, the preparation method of the present invention is simple, the raw materials are cheap, and the production cost is reduced; by pressing a multi-layer copper mesh on the porous copper surface and performing hydrophilic and hydrophobic modification on the surface, the bubble detachment rate and the boiling heat transfer coefficient are improved, and the heat flux density value corresponding to the peak value of the convective heat transfer coefficient is increased, thereby enhancing the heat exchange efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The SEM images of the powder-molded porous copper heat dissipation material prepared by the present invention are unmodified, hydrophilically modified, and hydrophobically modified; (a) comparative example 1 is unmodified, (b) comparative example 2 is hydrophilically modified, and (c) comparative example 3 is hydrophobically modified;

[0035] Figure 2 The contact angles of water droplets and surfaces taken in Comparative Examples 1, 2 and 3; (a) 50% porosity porous copper, (b) 50% porous copper after hydrophilic modification, (c) 50% porous copper after hydrophobic modification;

[0036] Figure 3Pool boiling heat transfer curves of samples prepared in comparative examples 1, 2 and 3 respectively; (a) curve of heat flux density changing with wall superheat, (b) curve of heat transfer coefficient changing with heat flux density;

[0037] Figure 4 The SEM images of the unmodified, hydrophilically modified, and hydrophobically modified improved powder-molded porous copper heat dissipation materials based on the surface composite copper mesh prepared by the present invention are shown in FIG. 1 ; (a) comparative example 4 is unmodified, (b) comparative example 5 is hydrophilically modified, and (c) example 1 is hydrophobically modified;

[0038] Figure 5 The contact angles of water droplets and surfaces taken in Comparative Example 4, Comparative Example 5 and Example 1; (a) 60-80 mesh-50%-1.5mm gradient porous copper, (b) hydrophilic modified 60 mesh-80 mesh-50%-1.5mm gradient porous copper, (c) hydrophobic modified 60 mesh-80 mesh-50%-1.5mm gradient porous copper;

[0039] Figure 6 Pool boiling heat transfer curves of samples prepared in Comparative Example 4, Comparative Example 5 and Example 1 respectively; (a) curve of heat flux density changing with wall superheat, (b) curve of heat transfer coefficient changing with heat flux density. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0041] Comparative Example 1

[0042] A method for preparing a powder-molded porous copper heat dissipation material comprises the following steps:

[0043] (1) Sodium chloride particles sieved through an 80-mesh sieve are used as pore-forming agents. The sodium chloride particles are placed in a vacuum drying oven at 50° C. and dried. After drying, 1.14 g of the sodium chloride particles are weighed and placed in a grinding jar together with electrolytic copper powder with a particle size of 5 μm and a mass of 4.73 g. The grinding jar is then placed in a planetary ball mill for thorough mixing to obtain a copper salt mixture. The ball milling time is 30 min and the rotation speed is 160 rpm.

[0044] (2) Weigh 5 g of the copper salt mixture and put it into a stainless steel mold, and press it into a powder-molded porous copper tablet.

[0045] The tablet was tested and found to have a thickness of 1.5 mm and a porosity of 50%. The boiling onset temperature (ONB) of the tablet reached 1.6°C and the heat transfer performance was up to 49407 W·m -2 ·K -1 , which is 3 times that of smooth copper under the same heat flux density, and 1.25-2 times that of foam copper under the same thickness.

[0046] Comparative Example 2

[0047] A method for preparing a surface-modified powder-molded porous copper heat dissipation material comprises the following steps:

[0048] Step (1) and step (2) are consistent with Comparative Example 1;

[0049] (3) After the hydrophilic surface of the pressed sheet prepared in step (2) is modified by chemical etching, the material is taken out and ultrasonically cleaned with deionized water and anhydrous ethanol in sequence. After the cleaning is completed, the material is placed in a drying oven at 50° C. for drying to obtain a hydrophilic surface-modified nanoporous copper heat dissipation material;

[0050] Hydrophilic surface modification steps: First, measure 200mL of deionized water and pour it into a clean beaker for later use, then weigh 20g of sodium hydroxide powder, carefully add it to the beaker and stir continuously to ensure that it is completely dissolved; secondly, weigh 2.7g of potassium persulfate powder, add it to the completely dissolved sodium hydroxide solution, and continue to stir with a glass rod until the solution is evenly mixed; after the solution is prepared, put the prepared tablet into the mixed solution, and place the entire beaker in a constant temperature water bath for water bath heating. The constant temperature water bath temperature is 70°C. When the surface of the composite copper mesh changes from the original brick red to black, it means that the hydrophilic modification is completed.

[0051] Comparative Example 3

[0052] A method for preparing a surface-modified powder-molded porous copper heat dissipation material comprises the following steps:

[0053] Step (1) and step (2) are consistent with Comparative Example 1;

[0054] (3) using a chemical etching method to sequentially perform hydrophilic surface modification and hydrophobic surface modification on the pressed sheet prepared in step (2), taking out the material and ultrasonically cleaning it with deionized water and anhydrous ethanol in sequence, and after the cleaning is completed, placing the material in a drying oven at 50° C. for drying to obtain a hydrophobic surface-modified nanoporous copper heat dissipation material;

[0055] The hydrophilic surface modification step remains consistent with Comparative Example 2.

[0056] Hydrophobic surface modification step: The material after hydrophilic surface modification was immersed in 0.1 mol / L stearic acid ethanol solution and allowed to stand for 4 hours.

[0057] from Figure 1 and Figure 2It can be seen that the hydrophilic modified alkaline oxidation treatment changes the microscopic morphology of the porous copper surface, making it rougher, which helps to improve the surface hydrophilicity of the porous copper. The hydrophobic porous copper surface generates a rough microstructure, so when a water droplet contacts the surface, due to the combined effect of low surface energy and surface roughness, it is difficult for the water droplet to spread on the porous copper surface, thus forming a larger contact angle and a smaller rolling angle, showing hydrophobicity.

[0058] from Figure 3 It can be seen that after surface modification, the boiling heat transfer performance of all samples has been improved. Among them, the surface modification has the most obvious improvement on powder-formed porous copper. The heat transfer characteristics are significantly enhanced after surface hydrophilic and hydrophobic modification. In the early stage of boiling, the hydrophobic surface shows a relatively superior heat transfer performance. When the heat flux density is 110000 W·m -2 When the heat transfer coefficient is about 1.8 times that of the unmodified surface, it reaches 76000 W·m -2 ·K -1 However, as the boiling process progresses, in the middle and late stages, the hydrophilic surface gradually shows its advantages, and its heat transfer performance gradually surpasses that of the hydrophobic surface. -2 When the heat transfer coefficient is about 1.5 times that of the unmodified surface, it reaches 55000 W·m -2 ·K -1 .

[0059] Comparative Example 4

[0060] A method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh comprises the following steps:

[0061] (1) Cut the copper mesh into a copper mesh disc with a diameter of 30 mm according to the specification requirements, then use anhydrous ethanol ultrasonic cleaning to remove oil stains, then use 0.1 mol / L hydrochloric acid to remove oxides, then rinse with deionized water and vacuum dry the copper mesh disc;

[0062] (2) Sodium chloride particles sieved through an 80-mesh sieve were used as pore-forming agents. The sodium chloride particles were placed in a vacuum drying oven at 50° C. and dried. After drying, 1.14 g of the sodium chloride particles were weighed and placed in a grinding jar together with electrolytic copper powder with a particle size of 5 μm and a mass of 4.73 g. The grinding jar was then placed in a planetary ball mill for thorough mixing to obtain a copper salt mixture. The ball milling time was 30 min and the rotation speed was 160 rpm.

[0063] (3) Weigh 5 g of the copper salt mixture and put it into a stainless steel mold. First, manually compact it to form a loose structure. Then, lay a layer of 80-mesh copper mesh and a layer of 60-mesh copper mesh on the loose structure from bottom to top. Finally, press it into a tablet by a tablet press. The tablet press is set to a pressure of 250 MPa and a holding time of 180 s.

[0064] (4) placing the pressed tablet obtained in step (3) into a tubular furnace for vacuum sintering to improve the structural strength of the pressed sample, with a heating rate of 10°C / min and a sintering temperature of 750°C; waiting for the tubular furnace to cool naturally to room temperature, then taking out the sample, placing the taken sample in an ultrasonic cleaning machine, first ultrasonically cleaning it with deionized water and anhydrous ethanol until no white particles are precipitated on the surface of the sample when cleaning with anhydrous ethanol; after cleaning, moving the sample to a drying oven for vacuum drying for 4 hours; after drying, weighing the sample mass using an electronic balance and comparing it with the mass of the electrolytic copper powder initially used in step (2); if the mass difference between the two is within 3%, the cleaning and drying steps are completed, otherwise, ultrasonic cleaning and drying treatments need to be continued until the quality requirements are met.

[0065] Comparative Example 5

[0066] A method for preparing a nanoporous copper heat dissipation material based on a composite copper mesh and surface modification, comprising the following steps:

[0067] Steps (1) to (4) are consistent with Comparative Example 4;

[0068] (5) after the hydrophilic surface modification of the improved powder-molded porous copper heat dissipation material of the surface composite copper mesh prepared in step (4) is performed by chemical etching, the material is taken out and ultrasonically cleaned with deionized water and anhydrous ethanol in sequence. After the cleaning is completed, the material is placed in a drying oven at 50° C. for drying to obtain a nanoporous copper heat dissipation material of a composite copper mesh with a hydrophilic surface modification;

[0069] The hydrophilic surface modification step remains consistent with Comparative Example 2.

[0070] Embodiment 1

[0071] A method for preparing a nanoporous copper heat dissipation material based on a composite copper mesh and surface modification, comprising the following steps:

[0072] Steps (1) to (4) are consistent with Comparative Example 4;

[0073] (5) using a chemical etching method to sequentially perform hydrophilic surface modification and hydrophobic surface modification on the improved powder-molded porous copper heat dissipation material of the surface composite copper mesh prepared in step (4), taking out the material and ultrasonically cleaning it with deionized water and anhydrous ethanol in sequence, and after the cleaning is completed, placing the material in a drying oven at 50° C. for drying to obtain a nanoporous copper heat dissipation material of a composite copper mesh with a hydrophobic surface modification;

[0074] The hydrophilic surface modification step is consistent with that of comparative example 2; and the hydrophobic surface modification step is consistent with that of comparative example 3.

[0075] from Figure 4 and Figure 5 It can be seen that the hydrophilic modified alkaline oxidation treatment changes the microscopic morphology of the porous copper surface, making it rougher, which helps to improve the surface hydrophilicity of the porous copper. The hydrophobic porous copper surface generates a rough microstructure, so when a water droplet contacts the surface, due to the combined effect of low surface energy and surface roughness, it is difficult for the water droplet to spread on the porous copper surface, thus forming a larger contact angle and a smaller rolling angle, showing hydrophobicity.

[0076] from Figure 6 It can be seen that the wall superheat of the hydrophilic surface and the hydrophobic surface at the starting point of boiling is not determined by a single factor, but is the result of the combined effect of the wettability of the sample surface and the micro-nano structure. This synergistic effect makes surfaces with different wettability exhibit different boiling heat transfer performance during the boiling process. Although surface modification significantly enhances the boiling heat transfer performance of powder-formed porous copper, the generation of a large number of bubbles hinders the flow of liquid between microstructures, affecting the timely replenishment of fresh liquid to the micro-liquid layer. Therefore, in comparison, the strengthening effect of hydrophilic and hydrophobic modification on the surface composite copper mesh powder-formed porous copper is relatively small, and at a heat flux density of 180,000 W·m -2 When the hydrophobic surface heat transfer coefficient is about 1.3 times that of the unmodified surface, it is 82909 W·m -2 ·K -1 .

Claims

1. A method for preparing a nanoporous copper heat dissipation material based on a composite copper mesh and surface modification. It is characterized in that The following steps are involved: (1) placing a certain mass of a copper salt mixture into a stainless steel mold, first manually compacting it to form a loose structure, then laying multiple layers of copper meshes of different meshes in order from small to large and from top to bottom on the loose structure to form a composite gradient copper mesh, and pressing and molding to obtain a pressed sheet; the copper salt mixture is prepared by mixing sodium chloride particles and electrolytic copper powder; (2) vacuum sintering, cleaning, and drying the pressed tablet obtained in step (1) in sequence to obtain an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh; (3) The improved powder-molded porous copper heat dissipation material based on the surface composite copper mesh prepared in step (2) is subjected to hydrophilic surface modification and hydrophobic surface modification in sequence by chemical etching, and finally cleaned and dried to obtain a nanoporous copper heat dissipation material based on the composite copper mesh and surface modification.

2. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1, It is characterized in that In step (1), the multiple layers of copper mesh with different mesh sizes are a layer of 60-mesh copper mesh and a layer of 80-mesh copper mesh.

3. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (3), the hydrophilic surface modification process is: a. Preparation of a hydrophilic modification solution: sodium hydroxide was added to deionized water to prepare a sodium hydroxide solution having a concentration of 0.1 g / mL, and potassium persulfate was added to the sodium hydroxide solution, and stirred until the solution was uniformly mixed to obtain a hydrophilic modification solution; The concentration of potassium persulfate in the solution is 13.5 g / L; b. The improved powder-molded porous copper heat dissipation material based on the surface composite copper mesh prepared in step (2) is immersed in a hydrophilic modification solution, and then heated in a water bath at 60-80°C for 60-80 minutes. When the surface of the composite copper mesh changes from the original brick red to black, it indicates that the hydrophilic modification is completed.

4. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (3), the hydrophobic surface modification process is: immersing the material after the hydrophilic surface modification in a 0.1 mol / L stearic acid ethanol solution and letting it stand for 4-5 hours.

5. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (3), the cleaning and drying process is as follows: after taking out the material from the stearic acid ethanol solution, ultrasonic cleaning is performed with deionized water and anhydrous ethanol in sequence. After the cleaning is completed, the material is placed in a drying oven at 50° C. for drying.

6. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (2), the pressed tablet is placed in a tubular furnace for vacuum sintering, the heating rate is 8-12°C / min, and the sintering temperature is 650-850°C.

7. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (1), the sodium chloride particles are sieved through an 80-mesh sieve; the sodium chloride particles are dried in a vacuum drying oven at 50° C.; the particle size of the electrolytic copper powder is 5 μm; and the mass ratio of the dried sodium chloride particles to the electrolytic copper powder is 1:(4-5).

8. The method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (1), the preparation process of the copper salt mixture is as follows: drying the sodium chloride particles and placing them together with the electrolytic copper powder into a grinding jar, and then placing the grinding jar in a planetary ball mill for thorough mixing; the ball milling time is 25-35 minutes, and the rotation speed is 150-180rpm; and the tablet press is pressed to obtain a tablet, the tablet press is set to a pressure of 240-280MPa, and the pressure holding time is 180-200s.

9. A method for preparing a nanoporous copper heat dissipation material based on a combination of a composite copper mesh and surface modification according to claim 1 or 2, It is characterized in that In step (1), the pretreatment process of the copper mesh is: the copper mesh is cut into copper mesh discs according to the specification requirements, and then the copper mesh discs are ultrasonically cleaned with anhydrous ethanol to remove oil stains, and then the oxides are removed with hydrochloric acid with a concentration of 0.1 mol / L, and then the copper mesh discs are rinsed with deionized water and vacuum dried.

10. A method for preparing a nanoporous copper heat dissipation material based on a composite copper mesh and surface modification obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Method for preparing copper heat dissipation material through electrolytic copper powder injection molding

    CN119819927A

  • Method for producing copper heat dissipation material by electrolytic copper powder injection molding

    CN119819927B