Method for preparing silver-coated aluminum powder with core-shell structure through direct chemical silver plating on surface of superfine aluminum powder

By controlling the silver complex ions and reaction temperature through a one-step chemical reduction method, the deposition rate and diffusion rate of silver atoms can be regulated, solving the problems of complex and uncontrollable silver-coated aluminum powder preparation process, achieving a high-efficiency and environmentally friendly silver coating effect, which is suitable for conductive and electromagnetic shielding materials.

CN118926524APending Publication Date: 2024-11-12KUNMING GAOJU TECH CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411032092.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing silver-coated aluminum powder preparation processes are complex, the reaction process is uncontrollable, the silver content is high, it is impossible to control the morphology and thickness of the silver deposition layer, and there are also environmental pollution problems.

Method used

By employing a one-step chemical reduction method, the deposition rate and diffusion rate of silver atoms can be controlled by adjusting the activity of silver complex ions and key parameters of the reaction system, thereby achieving control over the morphology and thickness of silver deposition on the surface of aluminum powder and preparing core-shell structured silver-coated aluminum powder.

Benefits of technology

It simplifies the preparation process, reduces costs, improves production efficiency and product purity, and achieves uniformity and density of silver deposition layers, making it suitable for conductive fillers, electromagnetic shielding materials, and catalytic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926524A_ABST
    Figure CN118926524A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing silver-coated aluminum powder with a core-shell structure through direct chemical silver plating on the surface of superfine aluminum powder, and belongs to the technical field of surface treatment. According to the method, the deposition rate of silver atoms and the diffusion rate of the silver atoms on the aluminum surface are indirectly regulated and controlled by strictly controlling the surface active sites of the superfine aluminum powder, the activity of silver complex ions and key technical parameters of a reaction system, so that the silver deposition morphology, the deposition thickness and the compactness on the surface of the aluminum powder are controlled. The method disclosed by the invention is simple and efficient in process, low in cost, simple and convenient to operate, environment-friendly and pollution-free, and has the advantages of high coating rate and uniform coating, and the prepared silver-coated aluminum powder can be used as a conductive filler, an electromagnetic shielding material and a catalytic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing silver-coated aluminum powder with a core-shell structure by direct chemical silver plating on the surface of ultrafine aluminum powder, and belongs to the technical field of surface treatment. Background Art

[0002] As a precious metal, silver has excellent electrical conductivity, thermal conductivity and corrosion resistance, but silver is expensive. Aluminum powder has a small density and a low price, but there is usually an oxide film on the surface of the aluminum powder, which affects its conductivity. If silver and aluminum are combined to prepare a silver-coated aluminum composite material, it can not only improve the conductivity, oxidation resistance and corrosion resistance of the aluminum powder, but also significantly reduce the cost of the material, greatly expanding its application field. At present, silver-coated aluminum powder is widely used in electronics, conductive coatings, electromagnetic shielding materials, catalysis and other fields. The preparation of silver-coated aluminum powder is usually prepared by chemical plating. Under the action of a reducing agent, the silver source is reduced to a silver element and deposited on an aluminum substrate. However, due to the strong activity of aluminum, the morphology of the surface deposited silver layer and the quality of the coating are basically uncontrollable. In order to better control the morphology of the surface silver deposition layer, the most reported preparation method is two-step silver plating or organic system silver plating.

[0003] The first step of the two-step silver plating method requires complex pre-treatment of aluminum powder, including surface modification, activation to form catalytic centers or pre-plating intermediate layers, etc., and then chemical silver plating is performed on the aluminum powder obtained by the pre-treatment to prepare silver-coated aluminum powder. Chinese patent publication number CN114700489A discloses "a preparation process of silver-coated aluminum powder and silver-coated aluminum powder". The aluminum powder is first surface modified by a silane coupling agent, and then the modified aluminum powder is chemically plated with copper-nickel to obtain copper-nickel aluminum powder, and then displacement silver plating is performed. The specific process flow is shown in Figure 1 This method not only has cumbersome pre-treatment and complex process, but also has difficult control over the entire reaction process, high cost and long time consumption, and is not suitable for large-scale production applications; Chinese patent publications CN102248159A, CN101927342A and CN111531168A respectively disclose methods for preparing silver-coated aluminum powder, firstly using acetone or sodium hydroxide solution to clean the grease on the surface of the aluminum powder, then chemically plating copper to obtain copper-coated aluminum powder, and finally using the copper-coated aluminum powder for displacement silver plating to obtain silver-coated aluminum powder. The process flow is shown in Figure 2 These methods avoid aluminum powder corrosion, but the process is cumbersome, the cost is high, the deposition process of the intermediate copper plating layer is uncontrollable, and the introduction of SO4 2- and [Cu(NH3)4] 2+ Impurity ions such as SO4 2- With Ag + It is easy to produce white precipitate of Ag2SO4, [Cu(NH3)4] 2+It is easy to adsorb on the copper surface, blocking the replacement reaction between copper and silver ions, and the quality of the final silver coating is difficult to control; in order to simplify the preparation process of aluminum-coated aluminum powder, Chinese patent publication number CN101983805A discloses "a method of chemically coating aluminum powder without silver oxide", using argon atomization to prepare aluminum powder, and storing aluminum powder in anhydrous ethanol under the protection of argon for chemical silver plating to prepare silver-coated aluminum powder. This method does not require the step of aluminum powder pretreatment, but the whole process of the reaction requires the introduction of argon to avoid aluminum powder oxidation, and the reaction conditions are very harsh, and the equipment requirements are high, and there are certain limitations; in addition, Chinese patent CN104325137A discloses a method for preparing silver-coated aluminum powder by a single replacement method, which simplifies the preparation process, but requires ammonium citrate and triisopropanolamine to form a double complexing agent to coordinate silver ions, which not only increases the cost and operation difficulty, but also the ratio of different double complexing agents will cause the uniformity and stability of the silver coating to be affected. Organic system silver plating refers to silver plating aluminum powder in an organic solvent. The organic solvent generally uses polyols or acetone as a solvent. The silver plating steps are simple, but organic matter is toxic and the cost of wastewater treatment is high. Japanese patent WO2014 / 156978A1 discloses a method for silver plating in an organic solvent. A mixture of water and isopropanol is used as a reaction solvent. The reaction temperature is 45°C. Aluminum powder is placed in a mixed solvent, and sodium hydroxide is added to etch the oxide film layer on the surface of aluminum. Then, a reducing agent and a silver complex solution are added in sequence to react to obtain silver-coated aluminum powder. However, the reaction time is long, and the long-term high-temperature reaction of the organic solvent will increase the viscosity of the solvent, making solid-liquid separation difficult.

[0004] In summary, the current research on aluminum powder silver plating mainly has the following difficulties:

[0005] (1) The pretreatment process of aluminum powder is complicated. At present, there is no method to remove the oxide film on the surface of aluminum powder without affecting the aluminum

[0006] Methods for determining powder surface quality;

[0007] (2) Aluminum is an amphoteric metal, and chemical coating requires a neutral plating environment. However, the current silver plating formula often has a high pH value, the plating solution is unstable during the preparation process, the silver coating is not dense, and the coating effect is poor.

[0008] (3) The current chemical plating formula for silver plating on the surface of aluminum powder requires a large amount of chemical raw materials, and a complex two-step silver plating process is used, and multiple silver platings are required. The silver content is high, which increases the cost.

[0009] (4) The surface activity of aluminum powders with different particle sizes varies greatly. Different silver plating conditions are required for aluminum powders with different activities. The two-step silver plating method is not universal for silver plating of aluminum powders with different particle sizes.

[0010] It can be seen that the existing silver-coated aluminum powder preparation process is not only complicated, but also causes certain pollution to the environment. Moreover, the reaction process is uncontrollable, and it is impossible to achieve the regulation of the morphology of the silver deposition layer and the thickness of the coating. It is urgent to provide a simplified, efficient, green and environmentally friendly silver-coated aluminum powder preparation method that can control the morphology and thickness of the coating on the aluminum powder surface. Summary of the invention

[0011] In view of the problems that the current preparation process of silver-coated aluminum powder is complicated, the reaction process is uncontrollable, the silver content is high, and the morphology and thickness of the silver deposition layer cannot be regulated, the present invention proposes a method for preparing a core-shell structure silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder. The method only needs to simply control the activity of silver complex ions and the key technical parameters of the reaction system to indirectly regulate the deposition rate of silver atoms and the diffusion rate of silver atoms on the surface of aluminum balls, thereby achieving the control of the silver deposition morphology and deposition thickness on the aluminum powder surface (see Figure 3 ). Compared with the traditional two-step method and organic system silver plating method, the method of the present invention has the advantages of simple and efficient process, no complicated pre-treatment process, only one-step reaction, low cost, simple operation, environmental protection and no pollution, and can achieve a high coating rate and uniform coating at a low silver content. The prepared silver-coated aluminum powder can be used as a conductive filler, electromagnetic shielding material or catalytic material.

[0012] The silver-coated aluminum powder of the present invention has a structure with ultrafine spherical aluminum particles as the core and a dense silver metal coating on the surface. The silver is plated by one-step chemical reduction. During the reaction, only an oxidant and a reductant participate in the reaction. The silver complex ions are directly reduced to silver element by electron transfer and deposited on the surface of the ultrafine aluminum powder. The surface of the ultrafine aluminum powder can be completely coated with the silver coating by one-step silver plating.

[0013] A method for preparing a core-shell structured silver-coated aluminum powder by directly chemically plating silver on the surface of ultrafine aluminum powder, wherein the silver-coated aluminum powder has ultrafine spherical aluminum particles as the core and a dense silver metal coating on the surface;

[0014] The specific steps of the preparation method are as follows:

[0015] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with the aluminum oxide film removed is added to an aqueous solution containing a dispersant, and stirred sufficiently to cause the dispersant to adsorb on the aluminum surface to form a protective layer, thereby obtaining an ultrafine aluminum powder suspension solution. The protective layer not only increases the wettability of the aluminum particles with the silver plating solution, but also effectively isolates the OH - The corrosion and dissolution of aluminum particles inhibits the hydrogen evolution side reaction during the silver plating process, thereby significantly improving the density of the silver plating layer;

[0016] (2) preparing a silver complex solution and a reducing agent solution: adding a silver nitrate solution to a complexing agent solution to form a complexing solution of silver ions, thereby obtaining a silver complexing solution; dissolving a reducing agent in deionized water to prepare a reducing agent solution;

[0017] (3) adding a silver complex solution dropwise: adding a reducing agent solution to a suspension of ultrafine aluminum powder to form a mixed solution, adding the silver complex solution to the mixed solution at a rate of 1 to 5 mL / min, maintaining the pH of the reaction system between 9 and 10, stirring the reaction at a temperature of 40 to 60° C. for 5 to 25 min, separating the solid from the liquid, washing the solid with deionized water and ethanol in turn to remove surface impurities, and vacuum or freeze-drying to obtain a silver-coated aluminum powder containing a dense silver coating; controlling the deposition amount of silver atoms and the diffusion rate of silver atoms on the surface of the aluminum powder by the reaction time and temperature to adjust the morphology and thickness of the silver deposition layer, thereby obtaining ultrafine silver-coated aluminum powders with different silver contents.

[0018] The particle size of the ultrafine aluminum powder in step (1) is 1 to 100 μm, preferably 1 to 10 μm, so as to maintain the high activity of the aluminum powder.

[0019] The concentration of the ultrafine aluminum powder suspension solution in step (1) is 15-100 g / L, and the dispersant can be selected from two types of non-ionic dispersants and natural dispersants, such as any one or more of xanthan gum, chitosan, gel, xylan, protein, gelatin, polyvinyl alcohol, polyethylene glycol, Tween 20, Tween 80, polyvinyl pyrrolidone, polyvinyl alcohol, etc., and the dispersant concentration is 0.2-1 g / L.

[0020] In the step (2), the molar ratio of silver nitrate to the complexing agent is 0.5-1:5-10, and the mass ratio of silver to the reducing agent is 0.5-1:0.3-2.

[0021] The complexing agent in step (2) is a polyhydroxy compound or an amino compound, such as triethanolamine, glycerol, sodium citrate, ethylenediaminetetraacetate, diethanolamine, triethylamine, diethylenetriamine, tetraethylenepentaamine or ammonia water, and the concentration of the complexing agent is 5-10 g / L.

[0022] The reducing agent in step (2) is a tartrate, such as sodium tartrate, potassium tartrate or potassium sodium tartrate, and the concentration of the reducing agent is 1.5-5 g / L.

[0023] During the reaction process of the present invention, the pH value of the system is maintained at 9-10 to ensure that the reaction process is mainly chemical plating, and the stability of the silver complex solution can also be ensured, which is conducive to forming a dense silver deposition layer.

[0024] The stirring rate of step (3) is 100-500 r / min, and vacuum drying or freeze drying (freeze drying) is used to avoid oxidation and agglomeration.

[0025] In step (3), the droplet addition rate is controlled to be 1 to 5 mL / min and the reaction temperature is 40 to 60° C., which can effectively adjust the deposition rate of silver atoms to be 0.02 to 0.1 mol·L -1·min, the diffusion rate of silver atoms on the surface of aluminum particles is 0.40~2.64mol·cm -1 ·min -1 to obtain a complete and dense silver deposition layer.

[0026] The core-shell structured silver-coated aluminum powder has an average particle size of preferably 1 to 10 microns and a silver content of 5 to 30%. It has a high coverage rate and a uniformly plated silver layer with good density and is suitable for conductive fillers, electromagnetic shielding materials and catalytic materials.

[0027] Preparation principle of silver-coated aluminum powder: The present invention uses potassium tartrate salts as a reducing agent and silver complex ions as an oxidant. Controlling the reaction pH can weaken the replacement reaction between the silver complex ions and the aluminum substrate, so that oxidation-reduction takes a dominant position. Secondly, during the deposition of silver, the silver atoms adsorbed on the aluminum surface may not always stay in the same position where the deposition occurs. On the contrary, due to the participation of surface diffusion, they can migrate to other sites on the aluminum substrate, which may change the growth pathway of the silver atoms and thus affect the final deposition morphology of the silver atoms. The most critical factor affecting diffusion is the reaction temperature. Therefore, the present invention can achieve a one-step preparation of a core-shell structured silver-coated aluminum powder by controlling the deposition and diffusion rate of silver atoms. The thermodynamics involved are as follows:

[0028] Reduction reaction:

[0029] [A g (NH3)2] + +e→A g +2NH3φ θ =0.373V

[0030] Oxidation reaction:

[0031]

[0032] Total electrode reaction and cell electromotive force:

[0033]

[0034] Overall redox reaction and total electromotive force:

[0035]

[0036] Based on the above thermodynamic analysis, when the reaction pH is greater than 9, the total potential of the redox reaction is 0.926V >> the replacement reaction cell electromotive force 0.203V. At this time, the redox reaction dominates.

[0037] The beneficial effects of the present invention are:

[0038] (1) The present invention strictly controls the dripping speed of silver complex ions and the reaction temperature of the system in the aqueous phase to prepare silver-coated aluminum powder by one-step chemical reduction, thereby simplifying the preparation process, avoiding the complex operation and potential pollution in the multi-step method, and improving the production efficiency and product purity;

[0039] (2) The present invention can control the dripping speed of the silver complex ion by a peristaltic pump, so that the silver deposition rate can be controlled. By controlling the reaction temperature and changing the mass of silver nitrate, the morphology and thickness of the silver deposition layer can be effectively controlled to avoid the problem of uneven silver layer.

[0040] (3) The method of the present invention is not only applicable to the silver plating of ultrafine aluminum powder of 1 to 10 μm, but also applicable to aluminum powder of more than 10 μm; it has wide applicability and flexibility, and meets the needs of different applications;

[0041] (4) The silver-coated aluminum powder prepared by the method of the present invention has uniform coating, excellent electrical conductivity and corrosion resistance, is suitable for the fields of electronics, conductive coatings, electromagnetic shielding and catalysis, and has significant technical and economic value. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is the flow chart of the first two-step method for preparing silver-coated aluminum powder;

[0043] Figure 2 This is the flow chart of the second two-step method for preparing silver-coated aluminum powder;

[0044] Figure 3 This is a flow chart for preparing the silver-coated aluminum powder of the present invention;

[0045] Figure 4 This is a SEM image of the silver-coated aluminum powder prepared in Example 1;

[0046] Figure 5 This is a SEM image of the silver-coated aluminum powder prepared in Example 2;

[0047] Figure 6 This is a SEM image of the silver-coated aluminum powder prepared in Example 3;

[0048] Figure 7 This is a SEM image of the silver-coated aluminum powder prepared in Example 4;

[0049] Figure 8 This is a SEM image of the silver-coated aluminum powder prepared in Example 5;

[0050] Fig. 9 This is the SEM image of the silver-coated aluminum powder prepared in Example 6. DETAILED DESCRIPTION

[0051] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0052] The silver-coated aluminum powder in the embodiment of the present invention has a structure with spherical aluminum particles as the core and a dense silver metal coating on the surface. One-step chemical reduction silver plating is adopted. During the reaction process, only an oxidant and a reductant participate in the reaction. Electron transfer directly reduces the complex ions of silver ions into silver element and deposits them on the surface of the aluminum powder. The surface of the aluminum powder can be completely coated by silver plating once. By strictly controlling the dripping speed of the silver complex ions and the reaction temperature of the system, the deposition rate of silver atoms and the diffusion rate of silver atoms on the surface of the aluminum spheres are indirectly regulated, thereby controlling the silver deposition morphology and deposition thickness on the surface of the aluminum powder.

[0053] Example 1: A method for preparing a core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder (see Figure 3 ), the specific steps are as follows:

[0054] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with a particle size of 40 μm is placed in a 0.8 g / L potassium fluoride solution for washing for 10 min to remove the aluminum oxide film layer, and the ultrafine aluminum powder after the film is removed is added to an aqueous solution containing a dispersant (polyvinyl pyrrolidone), and stirred to make the dispersant adsorb on the aluminum surface to form a protective layer to obtain an aluminum powder suspension; the aluminum powder concentration in the aluminum powder suspension is 17 g / L, and the dispersant concentration is 0.2 g / L;

[0055] (2) slowly adding silver nitrate solution into ammonia solution, stirring until transparent, and standing for 2 to 3 minutes to allow silver ions to fully complex with ammonia solution to prepare a silver ammonia solution; the molar ratio of silver nitrate to ammonia solution in the silver ammonia solution is 1:5; dissolving reducing agent potassium sodium tartrate in deionized water to obtain a reducing agent aqueous solution; the concentration of potassium sodium tartrate in the reducing agent aqueous solution is 2 g / L, and the mass ratio of silver to potassium sodium tartrate is 0.5:0.3;

[0056] (3) Add the reducing agent aqueous solution to the aluminum powder suspension to form a mixed solution. At a temperature of 40°C, use a peristaltic pump to add the silver ammonia solution dropwise to the mixed solution at a rate of 2 mL / min. The reduction rate of silver atoms is maintained at 0.02 mol·L -1 min, the diffusion rate of silver atoms on the aluminum surface is maintained at 0.5 mol·cm -1 ·min -1 , the pH value of the system was maintained at 9-10 and the reaction was stirred for 25 minutes (stirring rate was 300r / min); solid-liquid separation was performed, and surface impurities were removed by washing with deionized water and ethanol in turn, and the silver-coated aluminum powder was obtained by vacuum drying at a temperature of 40°C;

[0057] The silver content in the silver-coated aluminum powder of this embodiment is 17%. Figure 4,from Figure 4 It can be seen that the surface of the aluminum particles is covered with a dense silver film, and the average thickness of the silver shell is about 190nm.

[0058] Example 2: A method for preparing a core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder (see Figure 3 ), the specific steps are as follows:

[0059] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with a particle size of 40 μm is put into a 0.2 g / L sodium hydroxide solution for washing for 10 min to remove the aluminum oxide film layer, and the ultrafine aluminum powder after the film is removed is added to an aqueous solution containing a dispersant (Tween 20), and stirred to make the dispersant adsorb on the aluminum surface to form a protective layer to obtain an aluminum powder suspension; the aluminum powder concentration in the aluminum powder suspension is 30 g / L, and the dispersant concentration is 0.3 g / L;

[0060] (2) slowly adding a silver nitrate solution into an ammonia solution, stirring until transparent, and standing for 2 to 3 minutes to allow silver ions to fully complex with disodium ethylenediaminetetraacetate to prepare a silver complex solution; the molar ratio of silver nitrate to disodium ethylenediaminetetraacetate in the silver complex solution is 1:10; dissolving a reducing agent potassium tartrate in deionized water to obtain a reducing agent aqueous solution; the concentration of potassium tartrate is 5 g / L, and the mass ratio of silver in the silver complex solution to potassium sodium tartrate in the reducing agent aqueous solution is 1:2;

[0061] (3) Add the reducing agent aqueous solution to the aluminum powder suspension to form a mixed solution. At a temperature of 45°C, use a peristaltic pump to dropwise add the silver complex solution to the mixed solution at a rate of 2 mL / min. The reduction rate of silver atoms is maintained at 0.02 mol·L -1 min, the diffusion rate of silver atoms on the aluminum surface is maintained at 1 mol cm -1 ·min -1 , keeping the pH value of the system at 9-10 and stirring the reaction for 20 minutes (stirring rate is 500r / min); solid-liquid separation, the solid is washed with deionized water and ethanol in turn to remove surface impurities, and vacuum dried at a temperature of 40°C to obtain silver-coated aluminum powder;

[0062] The silver content in the silver-coated aluminum powder of this embodiment is 25%. The SEM image of the silver-coated aluminum powder is shown in FIG. Figure 5 ,from Figure 5 It can be seen that the silver deposition layer completely covers the aluminum particles, the silver plating is dense and has no leakage phenomenon, and the plating thickness is about 400nm.

[0063] Example 3: A method for preparing a core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder (see Figure 3 ), the specific steps are as follows:

[0064] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with a particle size of 20 μm is placed in a 1 g / L potassium fluoride solution for washing for 15 min to remove the aluminum oxide film layer, and the ultrafine aluminum powder after the film is removed is added to an aqueous solution containing a dispersant (gelatin), and stirred to make the dispersant adsorb on the aluminum surface to form a protective layer to obtain an aluminum powder suspension; the aluminum powder concentration in the aluminum powder suspension is 15 g / L, and the dispersant concentration is 0.5 g / L;

[0065] (2) slowly adding the silver nitrate solution to the triethanolamine solution, stirring until transparent, and standing for 2 to 3 minutes to allow the silver ions to fully complex with the triethanolamine to prepare a silver ion complex solution; the molar ratio of silver nitrate to triethanolamine is 0.8:8; dissolving potassium tartrate, a reducing agent, in deionized water to obtain a reducing agent aqueous solution; the concentration of potassium tartrate in the reducing agent aqueous solution is 3 g / L, and the mass ratio of silver to potassium tartrate is 0.3:2;

[0066] (3) Potassium tartrate aqueous solution was added to the aluminum powder suspension to form a mixed solution. At a temperature of 50°C, a peristaltic pump was used to add silver ammonia solution dropwise to the mixed solution at a rate of 3 mL / min. The reduction rate of silver atoms was maintained at 0.05 mol·L -1 min, the diffusion rate of silver atoms on the aluminum surface is maintained at 1.75 mol·cm -1 ·min -1 , keeping the pH value of the system at 9-10 and stirring the reaction for 20 min (stirring rate is 100 r / min); solid-liquid separation, washing with deionized water and ethanol in turn to remove surface impurities, freeze-drying for 4 h to obtain silver-coated aluminum powder;

[0067] The silver content in the silver-coated aluminum powder of this embodiment is 30%. The SEM image of the silver-coated aluminum powder is shown in FIG. Figure 6 ,from Figure 6 It can be seen that the coating is uniformly and densely coated on the aluminum surface, no unplated area is found, and the coating thickness is about 500nm.

[0068] Example 4: Preparation of core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder (see Figure 3 ), the specific steps are as follows:

[0069] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with a particle size of 5 μm is placed in a 0.3 g / L sodium hydroxide solution for washing for 10 min to remove the aluminum oxide film layer, and the ultrafine aluminum powder after the film is removed is added to an aqueous solution containing a dispersant (polyvinyl pyrrolidone), and stirred to make the dispersant adsorb on the aluminum surface to form a protective layer to obtain an aluminum powder suspension; the aluminum powder concentration in the aluminum powder suspension is 15 g / L, and the dispersant concentration is 1 g / L;

[0070] (2) slowly adding the silver nitrate solution to the tetraethylene pentaamine solution, stirring until transparent, and standing for 2 to 3 minutes to allow the silver ions to fully complex with the tetraethylene pentaamine, thereby preparing a silver ion complex solution; the molar ratio of silver nitrate to tetraethylene pentaamine is 1:8; dissolving the reducing agent sodium tartrate in deionized water to obtain a reducing agent aqueous solution; the concentration of the sodium tartrate is 5 g / L, and the mass ratio of silver to the sodium tartrate is 1:0.3;

[0071] (3) Add the reducing agent aqueous solution to the aluminum powder suspension to form a mixed solution. At a temperature of 55°C, use a peristaltic pump to add the silver ammonia solution dropwise to the mixed solution at a rate of 5 mL / min. The reduction rate of silver atoms is maintained at 0.1 mol·L -1 min, the diffusion rate of silver atoms on the aluminum surface is maintained at 2.5 mol·cm -1 ·min -1 , the pH value of the system was maintained at 9-10 and the reaction was stirred for 15 minutes (stirring rate was 200r / min); solid-liquid separation, the solid was washed with deionized water and ethanol in turn to remove surface impurities, and freeze-dried for 5 hours to obtain silver-coated aluminum powder;

[0072] The silver content in the silver-coated aluminum powder of this embodiment is 30%. The SEM image of the silver-coated aluminum powder is shown in FIG. Figure 7 ,from Figure 7 It can be seen that the silver coating completely covers the aluminum particles, the coating is dense and uniform, and the thickness of the silver layer is about 109nm.

[0073] Example 5: Preparation of core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder (see Figure 3 ), the specific steps are as follows:

[0074] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with a particle size of 3 μm is placed in a 0.2 g / L sodium hydroxide solution for washing for 10 min to remove the aluminum oxide film layer, and the ultrafine aluminum powder after the film is removed is added to an aqueous solution containing a dispersant (polyvinyl alcohol), and stirred to make the dispersant adsorb on the aluminum surface to form a protective layer to obtain an aluminum powder suspension; the aluminum powder concentration in the aluminum powder suspension is 15 g / L, and the dispersant concentration is 0.5 g / L;

[0075] (2) slowly adding the silver nitrate solution to the glycerol aqueous solution, stirring until transparent, and standing for 2 to 3 minutes to allow the silver ions to fully complex with the glycerol aqueous solution to prepare a silver ion complex solution; the molar ratio of silver nitrate to glycerol is 0.4:9; dissolving the reducing agent sodium tartrate in deionized water to obtain a reducing agent aqueous solution; the concentration of sodium tartrate is 3 g / L, and the mass ratio of silver to sodium tartrate is 1:0.3;

[0076] (3) Add the reducing agent aqueous solution to the aluminum powder suspension to form a mixed solution. Use a peristaltic pump to dropwise add the silver ammonia solution to the mixed solution at a rate of 5 mL / min at a temperature of 60°C. The reduction rate of silver atoms is maintained at 0.1 mol·L -1 min, the diffusion rate of silver atoms on the aluminum surface is maintained at 2.64 mol·cm -1 ·min -1 , the pH value of the system was maintained at 9-10 and the reaction was stirred for 20 minutes (stirring rate was 200r / min); solid-liquid separation, the solid was washed with deionized water and ethanol in turn to remove surface impurities, and freeze-dried for 5 hours to obtain silver-coated aluminum powder;

[0077] The silver content in the silver-coated aluminum powder of this embodiment is 25%. The SEM image of the silver-coated aluminum powder is shown in FIG. Figure 8 ,from Figure 8 It can be seen that the silver coating completely covers the aluminum particles, the coating is dense and uniform, and the thickness of the silver layer is about 78nm.

[0078] Example 6: Preparation of core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder (see Figure 3 ), the specific steps are as follows:

[0079] (1) Preparation of ultrafine aluminum powder suspension solution: ultrafine aluminum powder with a particle size of 10 μm is placed in a 0.3 g / L potassium fluoride solution for 10 min to remove the aluminum oxide film layer, and the ultrafine aluminum powder after the film is removed is added to an aqueous solution containing a dispersant (xanthan gum), and stirred to make the dispersant adsorb on the aluminum surface to form a protective layer to obtain an aluminum powder suspension; the aluminum powder concentration in the aluminum powder suspension is 15 g / L, and the dispersant concentration is 1 g / L;

[0080] (2) slowly adding the silver nitrate solution to the sodium citrate aqueous solution, stirring until transparent, and standing for 2 to 3 minutes to allow the silver ions to fully complex with the sodium citrate aqueous solution to prepare a silver ion complex solution; the molar ratio of silver nitrate to sodium citrate is 0.5:10; dissolving the reducing agent potassium sodium tartrate in deionized water to obtain a reducing agent aqueous solution; the concentration of potassium sodium tartrate is 2 g / L, and the mass ratio of silver to potassium sodium tartrate is 0.5:1;

[0081] (3) Add the reducing agent aqueous solution to the aluminum powder suspension to form a mixed solution. At a temperature of 50°C, use a peristaltic pump to add the silver ammonia solution dropwise to the mixed solution at a rate of 4 mL / min. The reduction rate of silver atoms is maintained at 0.08 mol·L -1 min, the diffusion rate of silver atoms on the aluminum surface is maintained at 2 mol·cm -1 ·min -1, the pH value of the system was maintained at 9-10 and the reaction was stirred for 20 minutes (stirring rate was 300r / min); solid-liquid separation, the solid was washed with deionized water and ethanol in turn to remove surface impurities, and freeze-dried for 5 hours to obtain silver-coated aluminum powder;

[0082] The silver content in the silver-coated aluminum powder of this embodiment is 25%. The SEM image of the silver-coated aluminum powder is shown in FIG. Fig. 9 ,from Fig. 9 It can be seen that the silver coating completely covers the aluminum particles, the coating is dense and uniform, and the thickness of the silver layer is about 300nm.

[0083] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder. It is characterized in that The silver-coated aluminum powder has ultrafine spherical aluminum particles as the core and a dense silver coating on the surface; The specific steps of the preparation method are as follows: (1) Preparation of ultrafine aluminum powder suspension solution: adding ultrafine aluminum powder with the aluminum oxide film removed into an aqueous solution containing a dispersant, and stirring the solution sufficiently to cause the dispersant to be adsorbed on the aluminum surface to form a protective layer, thereby obtaining an ultrafine aluminum powder suspension solution; (2) preparing a silver complex solution and a reducing agent solution: adding a silver nitrate solution to a complexing agent solution to form a complexing solution of silver ions, thereby obtaining a silver complexing solution; dissolving a reducing agent in deionized water to prepare a reducing agent solution; (3) adding a silver complex solution dropwise: adding a reducing agent solution to a suspension of ultrafine aluminum powder to form a mixed solution, adding the silver complex solution to the mixed solution at a rate of 1 to 5 mL / min, maintaining the pH of the reaction system between 9 and 10, stirring the reaction at a temperature of 40 to 60° C. for 5 to 25 min, separating the solid from the liquid, washing the solid with deionized water and ethanol in turn to remove surface impurities, and vacuum or freeze-drying to obtain a silver-coated aluminum powder containing a dense silver coating; controlling the deposition amount of silver atoms and the diffusion rate of silver atoms on the surface of the aluminum powder by the reaction time and temperature to adjust the morphology and thickness of the silver deposition layer, thereby obtaining ultrafine silver-coated aluminum powders with different silver contents.

2. The method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder according to claim 1, Features: The particle size of the ultrafine aluminum powder in step (1) is 1 to 100 μm.

3. The method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder according to claim 1, Features: The concentration of the ultrafine aluminum powder suspension solution in step (1) is 15-100 g / L, and the dispersant is one or more of xanthan gum, chitosan, gelatin, xylan, protein, gelatin, polyvinyl alcohol, polyethylene glycol, Tween 20, Tween 80, polyvinyl pyrrolidone, and polyvinyl alcohol, and the dispersant concentration is 0.2-1 g / L.

4. The method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder according to claim 1, Features: In step (2), the molar ratio of silver nitrate to complexing agent is 0.5-1:5-10, and the mass ratio of silver to reducing agent is 0.5-1:0.3-2.

5. The method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder according to claim 1, Features: The complexing agent in step (2) is triethanolamine, glycerol, sodium citrate, ethylenediaminetetraacetate, diethanolamine, triethylamine, diethylenetriamine, tetraethylenepentaamine or ammonia water, and the concentration of the complexing agent in the silver complexing solution is 5-10 g / L.

6. The method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder according to claim 1, Features: The reducing agent in step (2) is sodium tartrate, potassium tartrate or potassium sodium tartrate, and the concentration of the reducing agent in the reducing agent solution is 1.5-5 g / L.

7. The method for preparing core-shell structured silver-coated aluminum powder by direct chemical silver plating on the surface of ultrafine aluminum powder according to claim 1, Features: The stirring rate of step (3) is 100 to 500 r / min.

Citation Information

Cited By

  • Anti-yellowing high-gloss shimmering powder as well as preparation method and application thereof

    CN120888209A

  • Anti-yellowing high-light-shining powder, preparation method and application thereof

    CN120888209B

  • Multi-structure-layer flaky silver-coated aluminum powder, preparation method thereof and conductive rubber material

    CN121021931A