Palladium-copper bimetallic nanoparticle material, preparation method thereof and hydrogen sensing performance testing method

Preparation of palladium-copper bimetallic nanoparticles in aqueous solution by one-step method, solving the problems of cumbersome preparation methods and insufficient performance in the prior art, and achieving efficient and environmentally friendly hydrogen sensing materials with good selectivity and response speed .

CN118926539APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310532875.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the preparation method of palladium-copper bimetallic nanoparticle materials has cumbersome steps, poor repeatability, uneven size, uncontrollable morphology, and insufficient hydrogen sensing performance at room temperature.

Method used

The palladium and copper precursors were reduced in an aqueous solution by one-step method, and by changing the types and concentration of halides, a variety of palladium and copper bimetallic nanoparticles with controllable morphology and uniform size were prepared, simplifying the process and reducing raw material costs.

Benefits of technology

It realizes high selectivity, stability and mechanical strength of palladium-copper bimetallic nanoparticles, can quickly respond to hydrogen leakage at room temperature, is suitable for hydrogen detection, and has a simple process, environmentally friendly and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926539A_ABST
    Figure CN118926539A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of hydrogen sensing materials at room temperature, and discloses a palladium-copper bimetallic nanoparticle material, a preparation method thereof and a hydrogen sensing performance testing method. The method comprises the following steps: S1, mixing a palladium precursor solution, a surfactant solution, a halide solution and a copper precursor solution for reaction; and S2, mixing the reaction product obtained in the step S1 with a reducing agent solution for reaction. The material obtained by the method disclosed by the invention has excellent sensing performance, fast response time to hydrogen, relatively strong mechanical strength, hygrothermal stability and chemical stability, and can rapidly detect and respond to hydrogen leakage in the environment so as to ensure safe use of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of hydrogen sensing materials at room temperature, and in particular to a palladium-copper bimetallic nanoparticle material and a preparation method thereof, and a hydrogen sensing performance testing method. Background Art

[0002] At room temperature (RT), palladium (Pd) can react reversibly with H2 to catalytically dissociate hydrogen into hydrogen atoms, thereby forming palladium hydride (PdHx) with a higher resistivity than Pd. Quantitative detection of H2 is achieved by detecting the resistance signal based on the Pd sensor. However, poor hydrogen sensing response and slow reaction kinetics are often observed for single palladium metal. Even the response and recovery speed of hydrogen sensors based on nanoscale Pd-based hydrogen-sensitive materials are still insufficient. Compared with single metals, bimetallic nanoparticles exhibit better sensing performance due to the synergistic effect between metals. Therefore, the most effective method is to prepare bimetallic nanoparticles by introducing a second metal to reduce the amount of Pd in ​​hydrogen-sensitive materials and further improve the sensing performance. Metal Cu is abundant in reserves, much cheaper than Pd, and has the same face-centered cubic structure as Pd. PdCu bimetallic materials not only inherit the excellent performance of Pd in ​​catalytic dissociation of hydrogen, but also the presence of Cu atoms greatly improves the sensing performance. Therefore, researchers began to focus on the preparation of PdCu bimetallic nanoparticles.

[0003] The main preparation methods of Pd-based nanoparticles are electrodeposition, template method and chemical reduction method. The electrodeposition method has the disadvantages of poor repeatability and impure product composition, while the template method requires the preparation of templates in the early stage or the removal of templates in the later stage, and the operation is cumbersome; in comparison, the chemical reduction method is simple to operate, has good repeatability, and can obtain products with a single morphology and uniform size. At present, the seed method, i.e., the two-step method, is commonly used to prepare palladium nanoparticles. Not only does it require the pre-preparation of palladium nanoparticles with a certain morphology as seeds, but it is also necessary to add a morphology control agent in the subsequent reaction to guide or limit the growth of a specific crystal face, and then continue to grow on the basis of the original morphology to obtain palladium nanoparticles with different crystal faces. However, some special morphologies such as dendritic and mesoporous structures are mostly prepared by the two-step method (seed method) at high temperature, that is, Pd nanoparticles with a specific crystal face orientation are prepared in advance, and a certain amount of Pd particles after centrifugal washing are added to a solution containing a Cu precursor, and used as seeds to guide the growth of Pd particles on its surface. The seed method is not only cumbersome, but also rarely reported for the one-step synthesis of PdCu nanoparticles with special morphology. For the liquid phase reduction method, the synthesis of Pd-based bimetallic nanoparticles with a porous structure has been reported, but this method also has obvious defects, such as the non-aqueous organic solution environment and the need to use special precursor materials.

[0004] Therefore, there is an urgent need to provide a method that is simple, environmentally friendly and has low raw material prices. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of complicated steps, poor repeatability, uneven size, uncontrollable morphology, etc. in the prior art for preparing bimetallic nanoparticles, and to provide a palladium-copper bimetallic nanoparticle material and a preparation method thereof and a hydrogen sensing performance test method. The method adopts a one-step method to reduce palladium and copper precursors in an aqueous solution, and a variety of palladium-copper bimetallic nanoparticles with controllable morphology and uniform size can be prepared by changing the type of halide. The preparation method is simple and environmentally friendly, and the raw material price is low; the palladium-copper bimetallic nanoparticles provided by the present invention have good selectivity, stability, sensitivity and mechanical strength, and can be used for leakage and detection of hydrogen in an environment at room temperature.

[0006] In order to achieve the above object, the present invention provides a method for preparing a palladium-copper bimetallic nanoparticle material, which comprises the following steps:

[0007] S1, mixing a palladium precursor solution, a surfactant solution, a halide solution and a copper precursor solution for reaction;

[0008] S2, mixing the reaction product obtained in step S1 with a reducing agent solution to react.

[0009] Preferably, step S1 further comprises: mixing a palladium precursor solution and a surfactant solution, and then adding a halide solution and a copper precursor solution to the obtained mixed system, and reacting them under stirring conditions.

[0010] Preferably, in step S1, the reaction conditions include: the reaction temperature is 70-90°C.

[0011] Preferably, step S2 comprises: adding a reducing agent solution to the reaction product obtained in step S1, stirring and then reacting.

[0012] Preferably, the reaction conditions include: the reaction temperature is 50-100° C., and the reaction time is 1-12 h.

[0013] Preferably, the stirring conditions include: the stirring temperature is 70-90° C., and the stirring time is 1-5 min.

[0014] Preferably, step S2 comprises: adding a reducing agent solution to the reaction product obtained in step S1, stirring, reacting at 70-90° C. for 5-30 min, and then reacting at 50-100° C. for 0.5-12 h.

[0015] Preferably, the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 0.5-10:5-60:0.1-30:1:0.5-10, preferably 1-5:8-50:0.5-20:1:0.5-5.

[0016] Preferably, in step S1, the palladium precursor solution is selected from one or more of a palladium acetylacetonate solution, a palladium chloride solution, a palladium nitrate solution and a palladium sulfate solution.

[0017] Preferably, the concentration of the palladium precursor solution is 0.002M-0.05M, more preferably 0.0025M-0.03M, further preferably 0.0025M-0.02M.

[0018] Preferably, in step S1, the surfactant solution is selected from one or more of a CTAB solution, a CTAC solution, a PVP solution, a CPC solution and a SDBS solution.

[0019] Preferably, the concentration of the surfactant solution is 0.005M-0.06M, more preferably 0.01M-0.05M, further preferably 0.02M-0.03M.

[0020] Preferably, in step S1, the halide solution is selected from one or more of potassium fluoride solution, potassium chloride solution, potassium bromide solution, potassium iodide solution, sodium fluoride solution, sodium chloride solution, sodium bromide solution and sodium iodide solution, preferably one or more of potassium chloride solution, potassium bromide solution and potassium iodide solution.

[0021] Preferably, the concentration of the halide solution is 0.01M-0.2M, more preferably 0.02M-0.16M.

[0022] Preferably, in step S1, the copper precursor solution is selected from one or more of a copper acetylacetonate solution, a copper chloride solution, a copper nitrate solution and a copper ethyl sulfate solution.

[0023] Preferably, the concentration of the copper precursor solution is 0.005M-0.05M, more preferably 0.005M-0.03M, further preferably 0.005M-0.02M.

[0024] Preferably, in step S2, the reducing agent solution is selected from one or more of ascorbic acid solution, sodium borohydride solution and sodium hypophosphite solution.

[0025] Preferably, the concentration of the reducing agent solution is 0.005M-1M, more preferably 0.01M-0.06M, further preferably 0.01M-0.04M.

[0026] Preferably, the method further comprises: after the reaction in step S2 is completed, washing and drying the reaction product to obtain a palladium-copper bimetallic nanoparticle material.

[0027] Preferably, the drying conditions include: a drying temperature of 40-100° C., more preferably 50-80° C.; and a drying time of 12-36 h, more preferably 18-28 h.

[0028] The second aspect of the present invention provides a palladium-copper bimetallic nanoparticle material prepared by the method described in the first aspect, wherein the copper content is 5-50% by weight, preferably 25-50% by weight, based on the total weight of the palladium-copper bimetallic nanoparticle material.

[0029] Preferably, the average particle size of the palladium-copper bimetallic nanoparticle material is 100-150 nm.

[0030] The third aspect of the present invention provides a method for testing hydrogen sensing performance, the method comprising: placing a hydrogen sensing material in a sealed device, introducing a mixed gas containing hydrogen and a protective gas for reaction, and testing the resistance at different reaction times; the hydrogen sensing material is the palladium-copper bimetallic nanoparticle material described in the second aspect above.

[0031] Preferably, the concentration of hydrogen in the mixed gas is 0.02-2% by volume.

[0032] Preferably, the reaction conditions include: temperature of 15-30°C; time of 100-4000s, preferably 400-3500s.

[0033] The present invention provides a novel method for preparing palladium-copper bimetallic nanoparticle materials. The method adopts an aqueous one-step reduction method, wherein a palladium precursor and a copper precursor are simultaneously placed in an aqueous reaction solution, and then a reducing agent is added to reduce the palladium and copper. No seed crystals need to be prepared in advance, and palladium-copper bimetallic nanoparticles with different morphologies can be obtained by changing the type of halide added. The method is simple and easy to operate, environmentally friendly, and has low raw material prices. Moreover, the morphology is controllable, and nanoparticle materials with various morphologies can be obtained. Preferably, palladium-copper bimetallic nanoparticles of different sizes can be obtained by changing the concentration of the halide solution.

[0034] The material obtained by the method of the present invention has excellent sensing performance, fast response speed to hydrogen, strong mechanical strength, wet heat stability and chemical stability, and can quickly detect and respond to hydrogen leakage in the environment to ensure its safe use.

[0035] Compared with metal oxide-type hydrogen-sensitive materials, the new hydrogen-sensitive material provided by the present invention does not require heating, has low power consumption, good selectivity and fast response speed; the hydrogen-sensitive material provided by the present invention has a simple preparation process, good stability, low price, and is easy to be mass-produced and applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a curve of the resistance change over time of the material prepared in Example 9;

[0037] Figure 2 is a curve of the resistance change over time of the material prepared in Example 13;

[0038] Figure 3 is a curve showing the change of resistance of the material prepared in comparative example 3 over time;

[0039] Figure 4 is a SEM image of the material prepared in Example 1;

[0040] Figure 5 is a SEM image of the material prepared in Comparative Example 1;

[0041] Figure 6 is a SEM image of the material prepared in Comparative Example 2;

[0042] Figure 7 This is the SEM image of the material prepared in Comparative Example 3. DETAILED DESCRIPTION

[0043] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0044] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0045] The first aspect of the present invention provides a method for preparing a palladium-copper bimetallic nanoparticle material, the method comprising the following steps:

[0046] S1, mixing a palladium precursor solution, a surfactant solution, a halide solution and a copper precursor solution for reaction;

[0047] S2, mixing the reaction product obtained in step S1 with a reducing agent solution to react.

[0048] In the method provided in the first aspect of the present invention, a palladium precursor and a copper precursor are first mixed and reacted together in an aqueous phase, and a halide is added to regulate the morphology of the prepared nanoparticle material. Then, a reducing agent is added to reduce the palladium and copper precursors in one step, thereby obtaining bimetallic nanoparticle materials with different morphologies.

[0049] In the method described in the present invention, the order in which the palladium precursor solution, the surfactant solution, the halide solution and the copper precursor solution are mixed is not particularly limited, as long as they can react normally. In a specific embodiment, in step S1, the palladium precursor solution and the surfactant solution are mixed, and then the halide solution and the copper precursor solution are added to the obtained mixed system. In a specific embodiment, the reaction described in step S1 can be carried out under stirring conditions to promote the reaction. In a preferred embodiment, the specific process of step S1 includes: mixing the palladium precursor solution and the surfactant solution, and then adding the halide solution and the copper precursor solution to the obtained mixed solution, and reacting under stirring conditions.

[0050] In a specific embodiment, the reaction in step S1 can be carried out in a water bath or an oil bath. In a preferred embodiment, in step S1, the reaction conditions include: the reaction temperature can be 70-90°C. In the method of the present invention, the reaction time in step S1 is not particularly limited, and the reaction ends when the reaction system becomes a clear solution; in a preferred embodiment, the reaction time in step S1 is 10-30 minutes.

[0051] In the method of the present invention, the order of mixing the reaction product obtained in step S1 and the reducing agent solution is not limited. In a specific embodiment, the reaction product obtained in step S1 can be added to the reducing agent solution, or the reducing agent solution can be added to the reaction product obtained in step S1. In a specific embodiment, the mixture can be stirred for an appropriate time before the reaction step S1 is carried out, that is, the specific operation of step S2 includes: adding the reducing agent solution to the reaction product obtained in step S1 and stirring and then reacting. In a specific embodiment, the stirring temperature is the same as the reaction temperature in step S1, or it can be different. In a preferred embodiment, the stirring temperature can be 70-90°C; the stirring time can be 1-5min. In order to improve the reaction effect and obtain a bimetallic nanoparticle material with better performance, in a preferred embodiment, the reaction temperature in step S2 can be 50-100°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C; the reaction time can be 1-12h, for example, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h.

[0052] In the method of the present invention, in a more specific embodiment, the specific operation of step S2 includes: step S2 includes: adding a reducing agent solution to the reaction product obtained in step S1, stirring, reacting at 70-90°C for 5-30 minutes, and then reacting at 50-100°C for 0.5-12 hours. In a preferred embodiment, the stirring temperature can be 70-90°C; the stirring time can be 1-5 minutes.

[0053] In the method of the present invention, in order to obtain a palladium-copper bimetallic nanoparticle material with a fast response time to hydrogen, the amount ratio of each raw material needs to be controlled within an appropriate range. In a specific embodiment, the molar ratio of the amount of palladium precursor, surfactant, halide, copper precursor and reducing agent can be 0.5-10:5-60:0.1-30:1:0.5-10, preferably 1-5:8-50:0.5-20:1:0.5-5.

[0054] In the present invention, in a specific embodiment, the palladium precursor solution is prepared by mixing the palladium precursor with a hydrochloric acid solution.

[0055] In the method of the present invention, the palladium precursor solution can be a conventional choice in the art, as long as it can provide palladium for the bimetallic nanoparticle material. In a specific embodiment, in step S1, the palladium precursor solution is selected from one or more of acetylacetone palladium solution, palladium chloride solution, palladium nitrate solution and palladium sulfate solution. In a preferred embodiment, in step S1, the palladium precursor solution is a palladium chloride solution.

[0056] In the present invention, the concentration of the palladium precursor solution can be a concentration conventionally prepared in the art. In a specific embodiment, the concentration of the palladium precursor solution can be 0.002M-0.05M, preferably 0.0025M-0.03M, more preferably 0.0025M-0.02M, such as 0.0025M, 0.003M, 0.0035M, 0.004M, 0.005M, 0.006M, 0.008M, 0.01M, 0.012M, 0.013M, 0.014M, 0.015M, 0.016M, 0.017M, 0.018M, 0.019M or 0.02M.

[0057] In the method of the present invention, the surfactant is not particularly limited and can be any conventional surfactant in the art, as long as it has the function of regulating the morphology and dispersing the nanoparticles.

[0058] In the present invention, the surfactant solution can be an aqueous solution prepared by using water as a surfactant. In a specific embodiment, in step S1, the surfactant solution can be selected from one or more of CTAB (cetyltrimethylammonium bromide) solution, CTAC (cetyltrimethylammonium chloride) solution, PVP (polyvinylpyrrolidone) solution, CPC (cetylpyridinium chloride) solution and SDBS (sodium dodecylbenzenesulfonate) solution, preferably CPC (cetylpyridinium chloride) solution.

[0059] In the present invention, the concentration of the surfactant solution is not limited, as long as it can meet the usage ratio of the aforementioned raw materials. In a specific embodiment, the concentration of the surfactant solution is 0.005M-0.06M, preferably 0.01M-0.05M, more preferably 0.02M-0.03M, such as 0.02M, 0.021M, 0.022M, 0.023M, 0.024M, 0.025M, 0.026M, 0.027M, 0.028M, 0.029M or 0.03M.

[0060] In the method of the present invention, a variety of palladium-copper bimetallic nanoparticles with controllable morphology and uniform size can be prepared by changing the type of halide solution, and the morphology of the nanoparticles can be layered, dendritic, mesoporous, etc. Therefore, in the present invention, the type of the halide solution is not limited and can be a conventional choice in the art. In the present invention, the halide solution is an aqueous solution. In a specific embodiment, in step S1, the halide solution can be selected from one or more of potassium fluoride solution, potassium chloride solution, potassium bromide solution, potassium iodide solution, sodium fluoride solution, sodium chloride solution, sodium bromide solution and sodium iodide solution, preferably one or more of potassium chloride solution, potassium bromide solution and potassium iodide solution.

[0061] In the present invention, the size of the obtained palladium copper bimetallic nanoparticles can be adjusted by changing the concentration of the halide solution. In a specific embodiment, the concentration of the halide solution can be 0.01M-0.2M, preferably 0.02M-0.16M, such as 0.02M, 0.03M, 0.04M, 0.05M, 0.06M, 0.07M, 0.08M, 0.09M, 0.1M, 0.12M, 0.13M, 0.14M, 0.15M or 0.16M. In this article, the "M" refers to the unit mol / L.

[0062] In the method of the present invention, the copper precursor solution can be an aqueous solution prepared according to conventional methods in the art, and the type of the copper precursor solution is not limited, as long as it can provide copper for the bimetallic nanoparticle material. In a specific embodiment, in step S1, the copper precursor solution can be selected from one or more of acetylacetonate copper solution, copper chloride solution, copper nitrate solution and ethyl copper sulfate solution. In a preferred embodiment, in step S1, the copper precursor solution is a copper chloride solution.

[0063] In the present invention, in a specific embodiment, the concentration of the copper precursor solution can be 0.005M-0.05M, preferably 0.005M-0.03M, more preferably 0.005M-0.02M, for example 0.005M, 0.006M, 0.008M, 0.01M, 0.011M, 0.012M, 0.013M, 0.014M, 0.015M, 0.016M, 0.017M, 0.018M, 0.019M or 0.02M.

[0064] In the method of the present invention, in step S2, the reducing agent solution can be an aqueous solution prepared according to a conventional method in the art; the type of the reducing agent solution is not limited, as long as it can reduce palladium and copper. In a specific embodiment, in step S2, the reducing agent solution can be selected from one or more of ascorbic acid solution, sodium borohydride solution and sodium hypophosphite solution, preferably ascorbic acid solution.

[0065] In the present invention, in a specific embodiment, the concentration of the reducing agent solution can be 0.005M-1M, preferably 0.01M-0.06M, more preferably 0.01M-0.04M, for example 0.01M, 0.015M, 0.02M, 0.025M, 0.03M, 0.035M or 0.04M.

[0066] In the present invention, in order to improve the reducing effect of the reducing agent solution, in a preferred embodiment, the reducing agent solution is a freshly prepared reducing agent solution. In a specific operation, the reducing agent solution can be added dropwise to the reaction product obtained in step S1.

[0067] In the method of the present invention, in order to obtain pure and dry palladium-copper bimetallic nanoparticles, after the reaction in step S2 is completed, the reaction product is washed and dried to obtain palladium-copper bimetallic nanoparticle material. In a specific embodiment, after the reaction product in step S2 is cooled, it is washed alternately with deionized water and ethanol for several times, and then dried.

[0068] In the present invention, there is no particular limitation on the drying method, and room temperature evaporation or drying in a drying device can be used. In a specific embodiment, the drying conditions include: the drying temperature can be 40-100°C, preferably 50-80°C, such as 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C; the drying time can be 12-36h, preferably 18-28h, such as 18h, 19h, 20h, 21h, 22h, 23h, 24h, 25h, 26h, 27h or 28h.

[0069] The second aspect of the present invention provides a palladium-copper bimetallic nanoparticle material prepared by the method described in the first aspect. The palladium-copper bimetallic nanoparticle material provided by the present invention can be used as a hydrogen sensing material (hydrogen-sensitive material). The material has a fast response time to hydrogen, has strong mechanical strength, wet heat stability and chemical stability, can quickly detect and respond to hydrogen leakage in the environment to ensure its safe use, and at the same time, the method for preparing the hydrogen-sensitive material is simple and environmentally friendly, the raw material price is low and the process is simple.

[0070] In the palladium-copper bimetallic nanoparticle material of the present invention, the copper content can be 5-50% by weight, preferably 20-50% by weight, based on the total weight of the palladium-copper bimetallic nanoparticle material. The palladium-copper bimetallic nanoparticle material prepared by the method of the invention exists in the form of alloy bimetal. In the palladium-copper bimetallic nanoparticle material of the present invention, the average particle size of the prepared palladium-copper bimetallic nanoparticle material is 50-150nm.

[0071] The third aspect of the present invention provides a method for testing hydrogen sensing performance, the method comprising: placing a hydrogen sensing material in a sealed device, introducing a mixed gas containing hydrogen and a protective gas for reaction, and testing the resistance at different reaction times; the hydrogen sensing material is the palladium-copper bimetallic nanoparticle material described in the second aspect above.

[0072] In the specific testing process, a certain mass of palladium-copper bimetallic nanoparticles was placed in an agate mortar, and pine oil was added. After being fully ground into a slurry, it was evenly coated on a ceramic tube to prepare a component, which was then placed in a sealed device for testing.

[0073] In the hydrogen sensing performance test method of the present invention, the type of the sealed device is not limited, and it only needs to be a sealed device that can pass gas, such as a sealed chamber.

[0074] In the hydrogen sensing performance testing method of the present invention, in a specific embodiment, the concentration of hydrogen in the mixed gas can be 0.02-2 volume%, for example, 0.02 volume%, 0.05 volume%, 0.08 volume%, 0.1 volume%, 0.2 volume%, 0.3 volume%, 0.4 volume%, 0.5 volume%, 0.6 volume%, 0.7 volume%, 0.8 volume%, 0.9 volume%, 1 volume%, 1.2 volume%, 1.4 volume%, 1.5 volume%, 1.6 volume%, 1.8 volume% or 2 volume%.

[0075] According to the present invention, the protective gas may be a conventional choice in the art, and specifically, the protective gas may be nitrogen and / or air.

[0076] In the hydrogen sensing performance test method of the present invention, in a specific embodiment, the reaction conditions include: temperature of 15-30° C. (room temperature); time of 100-4000 s, preferably 400-3500 s.

[0077] In the present invention, the instrument used for hydrogen sensing performance testing is the CGS-8 intelligent gas sensitive analysis system produced by Elite Technology Co., Ltd.

[0078] The palladium-copper bimetallic nanoparticle material provided by the present invention is a hydrogen-sensitive material that directly addresses the leakage monitoring and safety issues of hydrogen, a new generation of clean energy. It can quickly detect and respond to hydrogen leakage in the environment at room temperature to ensure its safe use, and can be used in hydrogen production, hydrogenation, hydrogen storage and other hydrogen use links.

[0079] The present invention will be described in detail below by way of examples, but the protection scope of the present invention is not limited thereto. In the following examples and comparative examples, unless otherwise specified, all reagents used are commercially available.

[0080] In the embodiments and comparative examples of the present invention, the surfactant solution, the halide solution, the copper precursor solution, and the reducing agent solution are prepared by mixing the surfactant, the halide, the copper precursor, and the reducing agent with water respectively; the palladium precursor solution is prepared by mixing palladium chloride powder with dilute hydrochloric acid having a concentration of 37%.

[0081] Example 1

[0082] S1. Mix 10 mL of 0.02 M surfactant (CPC) solution with 4 mL of 0.005 M palladium precursor solution, then add 1 mL of 0.02 M halide (KCl) solution and 1 mL of 0.01 M copper precursor (CuCl2) solution, and then place the resulting mixed system in a water bath at 80 ° C and stir for reaction (about 20 min) until the solution is clear;

[0083] S2. Add 1 mL of a freshly prepared 0.02 M reducing agent (ascorbic acid) solution to the reaction product obtained in step S1, stir at 80 ° C for 2 min, then stop stirring, continue to react at 80 ° C for 10 min, and then react at 90 ° C for 6 h. After the reaction is completed, the reaction product is cooled and centrifuged, and then the obtained solid product is alternately washed 3 times with deionized water and ethanol, centrifuged after each washing, and dried to obtain a palladium-copper bimetallic nanoparticle material, wherein the drying temperature is 60 ° C, and the drying time is 24 h, wherein the molar ratio of the amount of palladium precursor, surfactant, halide, copper precursor and reducing agent is 2:20:2:1:2.

[0084] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 1 had a copper content of 22.5% by weight and a palladium content of 77.5% by weight;

[0085] The SEM characterization showed that Figure 4 As shown, the average particle size of the material prepared in Example 1 is 110 nm, and the morphology is cubic octahedron.

[0086] Example 2

[0087] The method of Example 1 is followed, except that the concentration of the palladium precursor solution is 0.0025 M, the concentration of the copper precursor (CuCl2) solution is 0.005 M, and the molar ratio of the palladium precursor, surfactant, halide, copper precursor and reducing agent is 2:40:4:1:4.

[0088] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 2 had a copper content of 25.5% by weight and a palladium content of 74.5% by weight;

[0089] According to SEM characterization, the average particle size of the material prepared in Example 2 is 100 nm, and the morphology is cubic octahedron.

[0090] Example 3

[0091] The method of Example 1 is followed, except that the concentration of the palladium precursor solution is 0.0075 M, the concentration of the copper precursor (CuCl2) solution is 0.015 M, and the molar ratio of the palladium precursor, surfactant, halide, copper precursor and reducing agent is 3:20:2:1.5:2.

[0092] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 3 had a copper content of 21.2% by weight and a palladium content of 78.8% by weight;

[0093] According to SEM characterization, the average particle size of the material prepared in Example 3 is 120 nm, and the morphology is cubic octahedron.

[0094] Example 4

[0095] The method of Example 1 is followed, except that the concentration of the palladium precursor (PdCl2) solution is 0.01 M, the concentration of the copper precursor (CuCl2) solution is 0.02 M, and the molar ratio of the palladium precursor, surfactant, halide, copper precursor and reducing agent is 2:10:1:1:1.

[0096] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 4 had a copper content of 20.3% by weight and a palladium content of 79.7% by weight;

[0097] According to SEM characterization, the average particle size of the material prepared in Example 4 is 135 nm, and the morphology is cubic octahedron.

[0098] Example 5

[0099] The method of Example 1 was followed, except that the surfactant was replaced by CTAB instead of CPC.

[0100] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 5 had a copper content of 22.3% by weight and a palladium content of 77.7% by weight;

[0101] According to SEM characterization, the average particle size of the material prepared in Example 5 is 120 nm and the morphology is cubic.

[0102] Example 6

[0103] The method of Example 1 was followed, except that the surfactant was replaced by CTAC instead of CPC.

[0104] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 6 had a copper content of 22.3% by weight and a palladium content of 77.7% by weight;

[0105] According to SEM characterization, the average particle size of the material prepared in Example 6 is 120 nm and the morphology is cubic.

[0106] Example 7

[0107] The method of Example 1 was followed, except that the surfactant was replaced by PVP instead of CPC.

[0108] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 7 had a copper content of 21.2% by weight and a palladium content of 78.8% by weight;

[0109] According to SEM characterization, the average particle size of the material prepared in Example 7 is 150 nm, and the morphology is irregular agglomerates.

[0110] Example 8

[0111] The method of Example 1 was followed, except that the surfactant was replaced by SDBS instead of CPC.

[0112] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 8 had a copper content of 21.9% by weight and a palladium content of 78.1% by weight;

[0113] According to SEM characterization, the average particle size of the material prepared in Example 8 is 135 nm, and the morphology is spherical particles.

[0114] Example 9

[0115] The method of Example 1 is followed, except that the concentration of the halide (potassium chloride) solution is 0.06 M, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:6:1:2.

[0116] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 9 had a copper content of 19.5% by weight and a palladium content of 80.5% by weight;

[0117] According to SEM characterization, the average particle size of the material prepared in Example 9 is 120 nm, and the morphology is cubic octahedron.

[0118] Example 10

[0119] The method of Example 1 is followed, except that the concentration of the halide (potassium chloride) solution is 0.1 M, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:10:1:2.

[0120] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 10 had a copper content of 19.6% by weight and a palladium content of 80.4% by weight;

[0121] According to SEM characterization, the average particle size of the material prepared in Example 10 is 125 nm, and the morphology is cubic octahedron.

[0122] Embodiment 11

[0123] The method of Example 1 is followed, except that the concentration of the halide (KCl) solution is 0.16 M, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:16:1:2.

[0124] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 11 had a copper content of 19.8% by weight and a palladium content of 80.2% by weight;

[0125] According to SEM characterization, the average particle size of the material prepared in Example 11 is 130 nm, and the morphology is cubic octahedron.

[0126] Example 12

[0127] The method of Example 1 was followed, except that the 0.02 M halide (KCl) solution was replaced with a 0.02 M potassium bromide (KBr) solution.

[0128] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 12 had a copper content of 25.5% by weight and a palladium content of 74.5% by weight;

[0129] According to SEM characterization, the average particle size of the material prepared in Example 12 is 115 nm, and the morphology is cubic octahedron.

[0130] Example 13

[0131] The method of Example 1 is followed, except that the 0.02 M halide (KCl) solution is replaced with a 0.06 M potassium bromide (KBr) solution, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:6:1:2.

[0132] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 13 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0133] According to SEM characterization, the average particle size of the material prepared in Example 13 is 115 nm, and the morphology is cubic octahedron.

[0134] Embodiment 14

[0135] The method of Example 1 is followed, except that the 0.02 M halide (KCl) solution is replaced with a 0.1 M potassium bromide (KBr) solution, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:10:1:2.

[0136] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 14 had a copper content of 23.4% by weight and a palladium content of 76.6% by weight;

[0137] According to SEM characterization, the average particle size of the material prepared in Example 14 is 125 nm, and the morphology is spherical particles.

[0138] Embodiment 15

[0139] The method of Example 1 is followed, except that the 0.02 M halide (KCl) solution is replaced with a 0.16 M potassium bromide (KBr) solution, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:16:1:2.

[0140] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 15 had a copper content of 23.3% by weight and a palladium content of 76.7% by weight;

[0141] According to SEM characterization, the average particle size of the material prepared in Example 15 is 130 nm, and the morphology is spherical particles.

[0142] Example 16

[0143] The method of Example 1 was followed, except that the 0.02 M halide (KCl) solution was replaced with a 0.02 M potassium iodide (KI) solution.

[0144] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 16 had a copper content of 47.3% by weight and a palladium content of 52.7% by weight;

[0145] According to SEM characterization, the average particle size of the material prepared in Example 16 is 120 nm, and the morphology is spherical particles.

[0146] Embodiment 17

[0147] The method of Example 1 is followed, except that the 0.02 M halide (KCl) solution is replaced with a 0.06 M potassium iodide (KI) solution, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:6:1:2.

[0148] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 17 had a copper content of 44.5% by weight and a palladium content of 55.5% by weight;

[0149] According to SEM characterization, the average particle size of the material prepared in Example 17 is 128 nm, and the morphology is spherical particles.

[0150] Embodiment 18

[0151] The method of Example 1 is followed, except that the 0.02 M halide (KCl) solution is replaced with a 0.1 M potassium iodide (KI) solution, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:10:1:2.

[0152] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 18 had a copper content of 44.5% by weight and a palladium content of 55.5% by weight;

[0153] According to SEM characterization, the average particle size of the material prepared in Example 18 is 128 nm, and the morphology is spherical particles.

[0154] Embodiment 19

[0155] The method of Example 1 is followed, except that the 0.02 M halide (KCl) solution is replaced with a 0.16 M potassium iodide (KI) solution, wherein the molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 2:20:16:1:2.

[0156] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 19 had a copper content of 44.3% by weight and a palladium content of 55.7% by weight;

[0157] According to SEM characterization, the average particle size of the material prepared in Example 19 is 135 nm, and the morphology is spherical particles.

[0158] Embodiment 20

[0159] The method of Example 1 was followed, except that in step S2, the reaction at 90° C. for 6 h was replaced by the reaction at 60° C. for 6 h.

[0160] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 20 had a copper content of 22.8% by weight and a palladium content of 77.2% by weight;

[0161] According to SEM characterization, the average particle size of the material prepared in Example 20 is 130 nm, and the morphology is cubic octahedron and spherical particles.

[0162] Embodiment 21

[0163] The method of Example 1 was followed, except that in step S2, the reaction was then carried out at 90° C. for 6 h instead of then reacting at 90° C. for 6 h.

[0164] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 21 had a copper content of 22.6% by weight and a palladium content of 77.4% by weight;

[0165] According to SEM characterization, the average particle size of the material prepared in Example 21 is 100 nm, and the morphology is an irregular cubic octahedron.

[0166] Embodiment 22

[0167] The method of Example 1 was followed, except that in step S2, the reaction at 90° C. for 6 h was replaced by the reaction at 100° C. for 6 h.

[0168] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 22 had a copper content of 22.5% by weight and a palladium content of 77.5% by weight;

[0169] According to SEM characterization, the average particle size of the material prepared in Example 22 is 95 nm, and the morphology is an irregular cubic octahedron.

[0170] Embodiment 23

[0171] The method of Example 1 was followed, except that in step S2, the reaction at 90° C. for 6 h was replaced by the reaction at 80° C. for 2 h.

[0172] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 23 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0173] According to SEM characterization, the average particle size of the material prepared in Example 23 is 100 nm, and the morphology is an irregular cubic octahedron.

[0174] Embodiment 24

[0175] The method of Example 1 was followed, except that in step S2, the reaction at 90° C. for 6 h was replaced by the reaction at 80° C. for 9 h.

[0176] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 24 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0177] According to SEM characterization, the average particle size of the material prepared in Example 24 is 110 nm and the morphology is cubic octahedron.

[0178] Embodiment 25

[0179] The method of Example 1 was followed, except that in step S2, the reaction at 90° C. for 6 h was replaced by the reaction at 80° C. for 12 h.

[0180] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 25 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0181] According to SEM characterization, the average particle size of the material prepared in Example 25 is 110 nm and the morphology is cubic octahedron.

[0182] Embodiment 26

[0183] The method of Example 1 is followed, except that in step S2, the drying temperature of 60° C. and the drying time of 24 h are replaced by the drying temperature of 40° C. and the drying time of 24 h.

[0184] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 26 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0185] According to SEM characterization, the average particle size of the material prepared in Example 26 is 110 nm, and the morphology is cubic octahedron and irregular cubic octahedron.

[0186] Embodiment 27

[0187] The method of Example 1 is followed, except that in step S2, the drying temperature of 60° C. and the drying time of 24 h are replaced by the drying temperature of 80° C. and the drying time of 24 h.

[0188] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 27 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0189] According to SEM characterization, the average particle size of the material prepared in Example 27 is 110 nm and the morphology is cubic octahedron.

[0190] Embodiment 28

[0191] The method of Example 1 is followed, except that in step S2, the drying temperature of 60° C. and the drying time of 24 h are replaced by the drying temperature of 100° C. and the drying time of 24 h.

[0192] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 28 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0193] According to SEM characterization, the average particle size of the material prepared in Example 28 is 110 nm and the morphology is cubic octahedron.

[0194] Embodiment 29

[0195] The method of Example 1 is followed, except that in step S2, the drying temperature of 60° C. and the drying time of 24 h are replaced by the drying temperature of 60° C. and the drying time of 12 h.

[0196] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 29 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0197] According to SEM characterization, the average particle size of the material prepared in Example 29 is 110 nm and the morphology is cubic octahedron.

[0198] Embodiment 30

[0199] The method of Example 1 is followed, except that in step S2, the drying temperature of 60° C. and the drying time of 24 h are replaced by the drying temperature of 60° C. and the drying time of 36 h.

[0200] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 30 had a copper content of 23.5% by weight and a palladium content of 76.5% by weight;

[0201] According to SEM characterization, the average particle size of the material prepared in Example 30 is 110 nm and the morphology is cubic octahedron.

[0202] Embodiment 31

[0203] The method of Example 1 is followed, except that the palladium precursor is replaced by palladium acetylacetonate from palladium chloride, and the copper precursor is replaced by copper acetylacetonate from copper chloride.

[0204] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 31 had a copper content of 24.5% by weight and a palladium content of 75.5% by weight;

[0205] According to SEM characterization, the average particle size of the material prepared in Example 31 is 120 nm and the morphology is cubic.

[0206] Embodiment 32

[0207] The method of Example 1 is followed, except that the palladium precursor is replaced by palladium sulfate instead of palladium chloride, and the copper precursor is replaced by copper sulfate instead of copper chloride.

[0208] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Example 32 had a copper content of 25.4% by weight and a palladium content of 74.6% by weight;

[0209] According to SEM characterization, the average particle size of the material prepared in Example 32 is 115 nm and the morphology is cubic.

[0210] Comparative Example 1

[0211] The method of Example 1 is followed, except that no surfactant (CPC) solution is added in step S1.

[0212] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Comparative Example 1 had a copper content of 36.6% by weight and a palladium content of 63.4% by weight;

[0213] The SEM characterization showed that Figure 5 As shown, the average particle size of the material prepared in Comparative Example 1 is 800 nm, and the morphology is spherical and rod-shaped particles.

[0214] Comparative Example 2

[0215] The method of Example 1 is followed, except that no halide (KCl) solution is added in step S1.

[0216] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Comparative Example 1 had a copper content of 26.8% by weight and a palladium content of 73.2% by weight;

[0217] The SEM characterization showed that Figure 6 As shown, the average particle size of the material prepared in Comparative Example 2 is 600 nm, and the morphology is spherical particles.

[0218] Comparative Example 3

[0219] The method of Example 1 is followed, except that in step S2, no reducing agent (ascorbic acid) solution is added.

[0220] Characterized by inductively coupled plasma mass spectrometry (ICP-MS), the material prepared in Comparative Example 1 had a copper content of 16.8% by weight and a palladium content of 83.2% by weight;

[0221] The SEM characterization showed that Figure 7 As shown, the average particle size of the material prepared in Comparative Example 3 is 500 nm, and the morphology is spherical particles.

[0222] Test Case

[0223] The materials prepared in the embodiment and the comparative example are used as hydrogen-sensitive materials to test the hydrogen sensing performance. The instrument used is the CGS-8 intelligent gas-sensitive analysis system of Elite Technology Co., Ltd. The test method includes: placing the materials prepared in the embodiment and the comparative example in a sealed cavity respectively, introducing a dry hydrogen and air mixed gas for reaction, wherein the concentration of hydrogen is 1% by volume, and all tests are measured at room temperature (25°C) for 3000s. The resistance variation curve over time is obtained, and the response time and recovery time are calculated according to the resistance variation curve over time, and the results are shown in Table 1.

[0224] The resistance variation curves of the materials prepared in Example 9, Example 13 and Comparative Example 3 over time are shown as follows: Figure 1 , Figure 2 and Figure 3 shown.

[0225] Response time is the time required for the resistance to reach 90% of the stable value from the initial value after contact with the target gas;

[0226] Recovery time is the time required for the sensor resistance to recover to 90% of the initial value when away from the target gas.

[0227] Table 1

[0228]

[0229]

[0230] It can be seen from Table 1 that the material prepared by the method of the present invention has excellent sensing performance, fast response speed to hydrogen, and short recovery time.

[0231] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing palladium-copper bimetallic nanoparticle material, characterized in that: The method comprises the following steps: S1, mixing a palladium precursor solution, a surfactant solution, a halide solution and a copper precursor solution for reaction; S2, mixing the reaction product obtained in step S1 with a reducing agent solution to react.

2. The method according to claim 1, characterized in that Step S1 comprises: mixing a palladium precursor solution and a surfactant solution, then adding a halide solution and a copper precursor solution to the obtained mixed system, and reacting them under stirring conditions; Preferably, in step S1, the reaction conditions include: the reaction temperature is 70-90°C.

3. The method according to claim 1 or 2, characterized in that: Step S2 comprises: adding a reducing agent solution to the reaction product obtained in step S1, stirring and reacting; Preferably, the reaction conditions include: the reaction temperature is 50-100°C, and the reaction time is 1-12h; Preferably, the stirring conditions include: the stirring temperature is 70-90° C., and the stirring time is 1-5 min.

4. The method according to claim 3, characterized in that Step S2 comprises: adding a reducing agent solution to the reaction product obtained in step S1, stirring, reacting at 70-90° C. for 5-30 minutes, and then reacting at 50-100° C. for 0.5-12 hours.

5. The method according to any one of claims 1 to 4, characterized in that: The molar ratio of the palladium precursor, the surfactant, the halide, the copper precursor and the reducing agent is 0.5-10:5-60:0.1-30:1:0.5-10, preferably 1-5:8-50:0.5-20:1:0.5-5.

6. The method according to any one of claims 1 to 5, characterized in that: In step S1, the palladium precursor solution is selected from one or more of a palladium acetylacetone solution, a palladium chloride solution, a palladium nitrate solution and a palladium sulfate solution; Preferably, the concentration of the palladium precursor solution is 0.002M-0.05M, more preferably 0.0025M-0.03M, further preferably 0.0025M-0.02M.

7. The method according to any one of claims 1 to 6, characterized in that: In step S1, the surfactant solution is selected from one or more of a CTAB solution, a CTAC solution, a PVP solution, a CPC solution and a SDBS solution; Preferably, the concentration of the surfactant solution is 0.005M-0.06M, more preferably 0.01M-0.05M, further preferably 0.02M-0.03M.

8. The method according to any one of claims 1 to 7, characterized in that: In step S1, the halide solution is selected from one or more of potassium fluoride solution, potassium chloride solution, potassium bromide solution, potassium iodide solution, sodium fluoride solution, sodium chloride solution, sodium bromide solution and sodium iodide solution, preferably one or more of potassium chloride solution, potassium bromide solution and potassium iodide solution; Preferably, the concentration of the halide solution is 0.01M-0.2M, more preferably 0.02M-0.16M.

9. The method according to any one of claims 1 to 8, characterized in that: In step S1, the copper precursor solution is selected from one or more of a copper acetylacetonate solution, a copper chloride solution, a copper nitrate solution and a copper ethyl sulfate solution; Preferably, the concentration of the copper precursor solution is 0.005M-0.05M, more preferably 0.005M-0.03M, further preferably 0.005M-0.02M.

10. The method according to any one of claims 1 to 9, characterized in that: In step S2, the reducing agent solution is selected from one or more of ascorbic acid solution, sodium borohydride solution and sodium hypophosphite solution; Preferably, the concentration of the reducing agent solution is 0.005M-1M, more preferably 0.01M-0.06M, further preferably 0.01M-0.04M.

11. The method according to any one of claims 1 to 10, characterized in that: The method further comprises: after the reaction in step S2 is completed, washing and drying the reaction product to obtain a palladium-copper bimetallic nanoparticle material; Preferably, the drying conditions include: a drying temperature of 40-100° C., more preferably 50-80° C.; and a drying time of 12-36 h, more preferably 18-28 h.

12. A palladium-copper bimetallic nanoparticle material prepared by the method according to any one of claims 1 to 11, characterized in that: Based on the total weight of the palladium-copper bimetallic nanoparticle material, the copper content is 5-50% by weight, preferably 20-50% by weight; Preferably, the average particle size of the palladium-copper bimetallic nanoparticle material is 100-150 nm.

13. A method for testing hydrogen gas sensing performance, characterized in that: The method comprises: placing a hydrogen sensing material in a sealed device, introducing a mixed gas containing hydrogen and protective gas for reaction, and testing the resistance at different reaction times; the hydrogen sensing material is the palladium-copper bimetallic nanoparticle material according to claim 12.

14. The method according to claim 13, characterized in that The concentration of hydrogen in the mixed gas is 0.02-2% by volume; Preferably, the reaction conditions include: temperature of 15-30°C; time of 100-4000s, preferably 400-3500s.