Preparation method of ferromagnetic shape memory alloy porous structure manufactured in composite mode

Through the composite manufacturing method, the porous structure of ferromagnetic shape memory alloy with bamboo grains is prepared by using laser impact-laser additive technology, which solves the problems of grain boundary limitation and insufficient mechanical properties, and achieves high magnetogenic strain and mechanical properties The improvement is suitable for low-cost and small-scale production.

CN118926547APending Publication Date: 2024-11-12WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411008986.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, due to grain boundary limitations, the magnetogenic strain value of ferromagnetic shape memory alloy polycrystalline materials is small, which greatly limits its shape memory effect, and it is impossible to prepare both 'bamboo' crystal grains in additive manufacturing. and porous structure, making it difficult to obtain a comprehensive performance with high mechanical properties and magneto-strain rate.

Method used

The composite manufacturing method is adopted, including configuring ferromagnetic shape memory alloy powder, manufacturing initial body-center cubic porous structure samples, measuring and constructing a three-dimensional porous structure model, preparing components through laser impact-laser additive composite manufacturing technology, and conducting thermal magnetic mechanical training , a porous structure with bamboo-like grains is formed.

Benefits of technology

It significantly reduces grain boundary limitations, enhances magnetogenic strain of polycrystalline alloys, improves shape memory effect, improves the mechanical properties of the alloys, realizes low-cost and small-scale production of parts, and expands the scope of engineering application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926547A_ABST
    Figure CN118926547A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a ferromagnetic shape memory alloy porous structure compositely manufactured. The preparation method comprises the following steps: preparing ferromagnetic shape memory alloy powder; manufacturing an initial body-centered cubic porous structure sample from the ferromagnetic shape memory alloy powder, and measuring to obtain the average crystal grain length and the average crystal grain width of columnar crystals of the initial body-centered cubic porous structure sample; constructing a three-dimensional porous structure model according to the measured average crystal grain length and average crystal grain width of the columnar crystal; the imported three-dimensional porous structure model is subjected to composite additive manufacturing in a laser shock-laser additive composite manufacturing mode, and a component is manufactured; and performing thermomagnetic mechanical training on the component. The formed alloy with the porous structure is obtained, the limitation of the grain boundary can be remarkably reduced, the magnetostrictive strain of the polycrystalline alloy is enhanced, and the shape memory effect is improved; beneficial microcosmic bamboo-like grains can be obtained, the mechanical property of the alloy is improved under the condition that large magnetostrictive strain is reserved, and the engineering application range of the alloy is greatly widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of ferromagnetic shape memory alloy porous structures, and in particular to a method for preparing a composite-manufactured ferromagnetic shape memory alloy porous structure. Background Art

[0002] Shape memory material is a special functional material that is responsive to stimulation and integrates sensing and driving. It can "memorize" a temporary shape under the stimulation of certain external conditions (light, heat, humidity, magnetic field, etc.) and can recover to its original shape. Shape memory alloys (SMA) are an important branch of shape memory materials. Due to their shape memory effect, superelasticity, high damping and other characteristics, they have great application potential in the automotive industry, aerospace, biomedicine, construction and other fields.

[0003] Shape memory alloys are divided into two categories: temperature-controlled shape memory alloys and ferromagnetic shape memory alloys. The recoverable strain of temperature-controlled shape memory alloys is induced by temperature and stress. Taking the representative Ni-Ti alloy as an example, the maximum strain energy currently available exceeds 13% (T≤20℃), and the response time takes a few seconds. The recoverable strain of ferromagnetic shape memory alloys can be induced by temperature, stress or magnetic field, among which Ni-Mn-Ga alloy is the most in-depth and representative one. It has the advantages of up to 15% maximum recoverable strain, adjustable phase transition temperature (-40℃-600℃), faster response speed (<1ms), and excellent elastic-thermal and magnetocaloric properties. Moreover, the strain induced by magnetic field can be easily realized at room temperature, with huge development potential and broad application prospects.

[0004] Magnetogenic strain (MFIS) is an important property of ferromagnetic shape memory alloys. It is a recoverable strain induced by a magnetic field and has long attracted much attention. Taking Ni-Mn-Ga based alloys as an example, the maximum MFIS obtained in the current study appears in single crystals. Sozinov et al. observed that about 12% MFIS was produced in the non-modulated martensite phase of Ni-Mn-Ga in a magnetic field of 1T at room temperature. However, single crystals grow slowly and are costly, and the preparation process is harsh, which is not conducive to large-scale production. Compared with single crystals, polycrystalline Ni-Mn-Ga is easier to process, but due to the limitation of grain boundaries and the anisotropic favorable orientation of twins in polycrystals, the strain of randomly textured polycrystals is very small, and MFIS is close to zero (0.002%). How to obtain a large MFIS in polycrystals is currently a difficulty in the study of Ni-Mn-Ga based ferromagnetic shape memory alloys.

[0005] To address this problem, Chmielus et al. developed a special casting process that uses liquid metal to infiltrate ceramic space support powder preforms to manufacture porous foam structured Ni-Mn-Ga polycrystals. By introducing pores similar in size to the grains to partially eliminate the constraints of grain boundaries, the MFIS value of polycrystalline Ni-Mn-Ga foam can reach 0.12%, which is significantly higher than that of dense block structured Ni-Mn-Ga polycrystals (0.002%); in addition, by introducing pores smaller than the grain size, the constraints can be further reduced, and the MFIS can be significantly increased to 2.0-8.7%, and remain stable for more than 200,000 cycles. This experiment proves that the porous structure can significantly improve the MFIS of Ni-Mn-Ga polycrystals, and in these Ni-Mn-Ga foams, a hierarchical structure with connecting nodes and pillars is formed, namely the so-called "bamboo-like" grains. Because the grain size spans the entire pillar width, the twin boundaries of these "bamboo-like" grains can move freely, resulting in a larger MFIS throughout the foam. Therefore, Ni-Mn-Ga polycrystalline materials with "bamboo-like" grains and porous structures have been shown to have the potential to achieve MFIS values ​​comparable to those of single crystals.

[0006] Based on the process properties of layered manufacturing and layer-by-layer stacking, metal additive manufacturing (AM) can produce complex metal structures with controllable arbitrary porosity. Therefore, AM technology has the potential to manufacture Ni-Mn-Ga components with excellent mechanical strength and large MFIS. At present, there have been studies exploring the method of using AM technology to manufacture Ni-Mn-Ga based ferromagnetic shape memory alloys with large MFIS:

[0007] 1. Binder jetting technology: Mostafei et al. used ball-milled Ni-Mn-Ga powder to make porous Ni-Mn-Ga parts, and the porosity of the parts was 24.08% and the MFIS was about 0.01%. Binder jetting technology is one of the methods for producing porous parts, but the size and distribution of the pores are difficult to control. In addition, this method requires necessary post-processing and cannot obtain good mechanical properties.

[0008] 2. Selective Laser Melting (SLM): Milleret et al. used the SLM process to fabricate Ni-Mn-Ga porous lattice structures. This technology can fabricate porous structures with controllable porosity, but no uniform “bamboo-like” grains were obtained in the fabricated samples, and thus no measurable MFIS was exhibited.

[0009] 3. Thin-wall printing technology: Laitinen et al. used SLM technology to prepare thin-walled Ni-Mn-Ga polycrystalline samples and heat-treated them. At room temperature, the largest single crystal grain of the polycrystalline sample with a 10M martensitic structure was measured to have an MFIS of 5.8%. This technology is mainly to obtain grains with larger MFIS similar to single crystals in polycrystalline, but the sample size that can be prepared by this method is small, which is not convenient for the actual production of polycrystalline Ni-Mn-Ga formed parts.

[0010] It can be seen that the current use of additive manufacturing technology to prepare ferromagnetic shape memory alloys mainly has the following difficulties:

[0011] (1) Due to the limitation of grain boundaries, the amount of magnetic strain that can be obtained in polycrystalline materials is small, which greatly limits its shape memory effect;

[0012] (2) It is impossible to prepare polycrystals with both “bamboo-like” grains and porous structures in AM, and thus it is difficult to obtain comprehensive properties with both high mechanical properties and magneto-induced strain rate. Summary of the invention

[0013] The present application provides a method for preparing a composite-manufactured porous structure of a ferromagnetic shape memory alloy, which can solve the technical problems existing in the prior art of preparing ferromagnetic shape memory alloys using additive manufacturing technology, namely, that the amount of magnetostrictive strain that can be obtained from polycrystalline materials is small due to the limitation of grain boundaries, which greatly limits its shape memory effect; and that it is impossible to prepare polycrystalline materials with both "bamboo-like" grains and porous structures in AM, and thus it is difficult to obtain comprehensive performance with both high mechanical properties and magnetostrictive strain rate.

[0014] In a first aspect, the present application provides a method for preparing a composite-made ferromagnetic shape memory alloy porous structure, comprising the following steps:

[0015] Step 1: preparing ferromagnetic shape memory alloy powder;

[0016] Step 2: using the configured ferromagnetic shape memory alloy powder to manufacture an initial body-centered cubic porous structure sample, and measuring and obtaining the average grain length and average grain width of columnar crystals of the initial body-centered cubic porous structure sample;

[0017] Step 3: Construct a three-dimensional porous structure model based on the measured average grain length and average grain width of the columnar crystals;

[0018] Step 4: Using a laser shock-laser additive manufacturing method to perform composite additive manufacturing on the imported three-dimensional porous structure model to obtain a component;

[0019] Step 5: Perform thermal magnetic mechanical training on the component to obtain a composite ferromagnetic shape memory alloy porous structure device.

[0020] In combination with the first aspect, in one embodiment, in step 1, the ferromagnetic shape memory alloy selected is a Ni-Mn-Ga alloy, and the element ratio in the ferromagnetic shape memory alloy powder is as follows: Ni is 49 wt% - 51 wt%, Mn is 28 wt% - 32 wt%, and Ga is 19 wt% - 21 wt%.

[0021] In combination with the first aspect, in one embodiment, in step 2, the porosity of the initial body-centered cubic porous structure sample is 10% - 60%.

[0022] In combination with the first aspect, in one embodiment, in step 2, the configured ferromagnetic shape memory alloy powder is used to manufacture the initial body-centered cubic porous structure sample by selective laser melting technology.

[0023] In combination with the first aspect, in one embodiment, in the selective laser melting technology, the laser power is 60 W - 100 W, the scanning speed is 250 mm / s - 650 mm / s, and the scanning spacing is 50 μm - 100 μm.

[0024] In combination with the first aspect, in one embodiment, in step 2, a conventional cubic porous structure sample is manufactured by electron beam selective melting technology or direct laser forming technology or arc additive manufacturing technology.

[0025] In combination with the first aspect, in one embodiment, step 3 specifically includes the following steps:

[0026] According to the measured average grain length and average grain width of the columnar crystals, the parameter setting constraints of a single lattice of the following three-dimensional porous structure model are constructed:

[0027] c = (0.90 - 0.99)L; and,

[0028] Both f1 and f2 are less than D or f1f2 < D 2 ; and,

[0029] ab < f1f2; and,

[0030] f3 = (0.10 - 0.45)c;

[0031] In the formula, a, b, and c are the lengths of the struts in the x direction, y direction, and z direction of a single lattice respectively, f1, f2, and f3 are the widths of the struts in the x direction, y direction, and z direction respectively, L is the average grain length, and D is the average grain width;

[0032] Based on the parameter setting constraints of a single lattice of the constructed three-dimensional porous structure model, the three-dimensional porous structure model is set.

[0033] In combination with the first aspect, in one embodiment, the method of performing composite additive manufacturing on the imported three-dimensional porous structure model by laser shock-laser additive manufacturing to obtain a component specifically includes the following steps:

[0034] Perform two-dimensional slicing and layering on the constructed three-dimensional porous structure model to obtain a model slicing and layering file;

[0035] Import the model slice layering file and generate the slice scanning path;

[0036] According to the model slicing and layering file, the imported three-dimensional porous structure model is processed layer by layer by composite additive manufacturing using a preparation method that alternates additive manufacturing and interlayer laser shock until the entire component is completed.

[0037] In combination with the first aspect, in one embodiment, the three-dimensional porous structure model is subjected to composite additive manufacturing processing layer by layer by using a preparation method of alternating additive manufacturing and interlayer laser shock according to the model slice layer file until the entire component is completed, specifically including the following steps:

[0038] Perform additive processing on the first layer of two-dimensional slices and layers of the imported three-dimensional porous structure model to obtain the required working conditions of laser shock for the current layer of two-dimensional slices and layers;

[0039] If laser shock is required, the layer is laser shocked;

[0040] If laser shock is not required, laser shock is not performed and the additive processing is continued on the next model layer;

[0041] The above steps are repeated until the composite additive manufacturing processing of all two-dimensional slices and layers of the imported three-dimensional porous structure model is completed to obtain a component.

[0042] In combination with the first aspect, in one embodiment, the manufactured component is cycled between martensite and austenite states under a rotating magnetic field, and the component is subjected to thermomagnetic mechanical training and cycled between martensite and austenite states under a rotating magnetic field.

[0043] The beneficial effects brought by the technical solution provided by the embodiment of the present application include at least:

[0044] (1) The present application adopts an additive manufacturing method in the process of processing and manufacturing ferromagnetic shape memory alloys to obtain a formed alloy with a porous structure, which can significantly reduce the restriction of grain boundaries, enhance the magnetostrictive strain of polycrystalline alloys, and improve the shape memory effect;

[0045] (2) The present application adds laser shock to the process of additive manufacturing of ferromagnetic shape memory alloys, which can obtain beneficial microscopic bamboo-like grains and improve the mechanical properties of the alloy while retaining large magneto-induced strain, greatly expanding its engineering application range;

[0046] (3) Compared with other manufacturing methods, the present invention can process and manufacture parts with complex geometric structures, realize rapid free forming without molds, and has a short part manufacturing cycle, small machining allowance, high material utilization rate, and can realize low-cost small-batch production of parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 is a schematic diagram of the initial body-centered cubic structure;

[0048] Figure 2 (a) is a schematic diagram of a single unit cell structure; Figure 2 (b) is a schematic diagram of the parameters of the normal viewing angle of a single unit cell; Figure 2 (c) is a schematic diagram of the parameters of a single unit cell from a top-down angle;

[0049] Figure 3 (a) is a schematic diagram of the lattice structure used in the laser shock path on the columnar crystal proposed in this application; Figure 3 (b) is a three-dimensional model diagram of a porous structure provided in an embodiment of the present application;

[0050] Figure 4 This is a flow chart of a method for preparing a composite ferromagnetic shape memory alloy porous structure according to an embodiment of the present application.

[0051] Figure 5 (a) is a macroscopic photograph of the composite fabricated object of the sample; Figure 5 (b) is a SEM photograph of the composite fabricated sample. DETAILED DESCRIPTION

[0052] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0053] The terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices. The terms "first", "second" and "third" are used to distinguish different objects, etc., and do not represent a sequence, nor do they limit "first", "second" and "third" to different types.

[0054] In the description of the embodiments of the present application, "exemplary", "for example" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary", "for example" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary", "for example" or "for example" is intended to present related concepts in a specific way.

[0055] In the description of the embodiments of the present application, unless otherwise specified, “ / ” means or, for example, A / B can mean A or B; the “and / or” in the text is merely a description of the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In addition, in the description of the embodiments of the present application, “multiple” refers to two or more than two.

[0056] In some processes described in the embodiments of the present application, multiple operations or steps that appear in a specific order are included, but it should be understood that these operations or steps may not be executed in the order in which they appear in the embodiments of the present application or in parallel, and the sequence number of the operation is only used to distinguish the different operations, and the sequence number itself does not represent any execution order. In addition, these processes may include more or fewer operations, and these operations or steps may be executed in sequence or in parallel, and these operations or steps may be combined.

[0057] In order to make the objectives, technical solutions and advantages of the present application clearer, the implementation methods of the present application will be further described in detail below with reference to the accompanying drawings.

[0058] The present application embodiment provides a method for preparing a composite ferromagnetic shape memory alloy porous structure, such as Figure 4 As shown, the following steps are included:

[0059] Step 1: Prepare ferromagnetic shape memory alloy powder with appropriate proportion; the ferromagnetic shape memory alloy selected in this application is Ni-Mn-Ga alloy, and the proportions of each element in the mixed powder are: Ni: 49wt%-51wt%, Mn: 28wt%-32wt%, Ga: 19wt%-21wt%.

[0060] Step S2: Select a suitable additive manufacturing process and its parameters to manufacture the configured ferromagnetic shape memory alloy powder into Figure 1 A series of initial body-centered cubic porous structure samples with porosity ranging from 10% to 60% are shown. The initial body-centered cubic porous structure samples are conventional porous structure samples. The average grain length L and average grain width D of columnar crystals of the initial body-centered cubic porous structure samples are measured to obtain.

[0061] like Figure 2 As shown in (a), the lengths of the pillars in a single lattice of the three-dimensional porous structure model are a, b, c, and the widths are f1, f2, and f3, respectively. According to the measured average grain length L and width D of the columnar crystals, the parameters of each pillar in a single lattice of the three-dimensional porous structure model must satisfy the following parameter setting constraints:

[0062] (1) c = (0.90-0.99) L;

[0063] (2) f1 and f2 are both less than D or f1f2 <D 2 ;

[0064] (3)ab <f1f2;

[0065] (4) f3 = (0.10-0.45) c;

[0066] The porosity σ of the prepared initial body-centered cubic porous structure sample was calculated according to the following formula:

[0067]

[0068] Wherein, a, b, and c are the length of the x-direction pillar, the length of the y-direction pillar, and the length of the z-direction pillar in a single lattice, respectively; f1, f2, and f3 are the width of the x-direction pillar, the width of the y-direction pillar, and the width of the z-direction pillar, respectively.

[0069] The porosity of the initial body-centered cubic porous structure sample obtained by calculation is between 10% and 30%.

[0070] Examples of values ​​for each parameter are shown in Table 1:

[0071] Table 1 Example of parameter values ​​of columnar crystals of initial body-centered cubic porous structure samples

[0072] serial number a b c <![CDATA[f1]]> <![CDATA[f2]]> <![CDATA[f3]]> σ 1 0.6D 0.7D 0.91L 0.9D 0.7D 0.41L 13.79% 2 0.7D 0.6D 0.92L 0.8D 0.8D 0.38L 14.15% 3 0.5D 0.8D 0.93L 0.7D 1.1D 0.34L 12.85% 4 0.8D 0.5D 0.94L 0.6D 1.2D 0.31L 12.64% 5 0.6D 0.6D 0.95L 0.5D 0.8D 0.28L 18.06% 6 0.8D 0.4D 0.96L 0.7D 0.9D 0.24L 13.13% 7 0.4D 0.8D 0.97L 0.9D 1.0D 0.20L 11.34% 8 0.9D 0.7D 0.98L 1.0D 0.7D 0.17L 20.18% 9 0.7D 0.9D 0.99L 1.2D 0.6D 0.13L 19.54%

[0073] Step S3: According to the above-measured average grain length L and columnar average grain width D, the required parameters a, b, c, f1, f2, and f3 are set to construct a structure having the following characteristics: Figure 3 The three-dimensional porous structure model shown in (a);

[0074] Step S4: Import the constructed model and set the additive manufacturing and laser shock programs. Figure 3 As shown in (b), the laser impact path is designed. The lattice structure shown in the figure can be divided into three parts: nodes, columns, and horizontal columns. The nodes are between columns. The nodes in the horizontal direction are connected by horizontal columns, and the nodes in the vertical direction are connected by columns.

[0075] Step S5: Additive manufacturing is started. During the manufacturing process, additive manufacturing and interlayer laser shock are used in an alternating preparation method. After each layer of additive manufacturing is completed, it is determined whether the layer needs to be laser shocked. If laser shock is required, the designated area is shocked; if laser shock is not required, the next layer of additive manufacturing is continued until the entire component is completed. Finally, "bamboo-shaped" grains composed of columnar crystals in the column and cross column parts and fine equiaxed crystals in the node part are formed; or "bamboo-shaped" grains composed of columnar crystals in the column part and fine equiaxed crystals in the node and cross column part are formed. During the manufacturing process, laser shock is applied to the node part, laser shock is not applied to the column part, and laser shock can be applied to the cross column part according to the specific situation. For the laser shock area, additive manufacturing and interlayer laser shock are used in an alternating preparation method, that is, after each N layers of additive manufacturing (N is a positive integer), m times (m is a positive integer) of laser shock are performed.

[0076] Step S6: Perform thermomechanical training on the component.

[0077] <Example 1>

[0078] Step 1: Prepare Ni-Mn-Ga alloy powder, the ratio of each element in the mixed powder of the alloy used is: Ni: 50wt%, Mn: 28.2wt%, Ga: 21.8wt%.

[0079] Step 2: A series of conventional body-centered cubic porous structure samples were manufactured using laser selective melting technology, with the target porosity set to 10%-60%, the laser power to 60W-100W, the scanning speed to 250mm / s-650mm / s, and the scanning spacing to 50μm-100μm. The length and width of the columnar crystals of samples with different porosities were measured, and the average length of the columnar crystals of all samples was calculated to be L = 0.86mm, and the average width was D = 0.55mm.

[0080] Step 3: According to the above D and L, set a series of a, b, c, f1, f2, f3 (values ​​are shown in Table 2 below, unit: mm) to construct a 10×10×10mm 3 3D model of the lattice structure with a constant powder layer thickness of 25 μm.

[0081] Table 2 List of a series of unit cell parameters set according to the average length and width of columnar crystals obtained by calculation in Implementation 1 (unit: mm)

[0082]

[0083]

[0084] Figure 5 The macroscopic and SEM photos of the composite fabricated product of sample No. 8 in Table 2 are given.

[0085] Step 4: Slice and layer the model in two dimensions, import the model slice and layer file into the additive manufacturing software, and generate the slice scanning path. The above-mentioned porous structure model is manufactured by laser selective melting technology, where the laser power is 60W-100W, the scanning speed is 250mm / s-650mm / s, and the scanning spacing is 50μm-100μm.

[0086] Step 5: Set the laser shock action path to shock only the node area and not the rest of the area, with the laser wavelength of 1064nm, pulse width of 9ns, laser energy of 2J-6J, and spot diameter of 1mm. Laser shock is performed once after adding two layers of material (laser shock).

[0087] Step 6: Start the manufacturing of porous alloy components according to the preset parameters and paths. After the current layer is added, determine whether there is an impact area that needs interlayer laser shock according to the slice file. If laser shock is required, shock the node area once; if laser shock is not required, continue to add material.

[0088] Step 7. The manufactured component is subjected to thermomagnetic mechanical training, cycling between the martensite and austenite states in a rotating magnetic field of 0.97 T for 15 cycles.

[0089] Step 8. End.

[0090] <Example 2>

[0091] Step 1: Prepare Ni-Mn-Ga alloy powder, the ratio of each element in the mixed powder of the alloy used is: Ni: 49.3wt%, Mn: 31.2wt%, Ga: 19.0wt%.

[0092] Step 2: Use electron beam selective melting technology to manufacture conventional body-centered cubic porous structure samples, set the target porosity to 10%-60%, set the scanning line spacing of the mixed powder preheating scan to 1.0 mm, and the scanning speed to (1.0-3.5)×10 4 mm / s, scanning current is 25A, electron beam deflection speed is 150mm / s-350mm / s, and electron beam scanning line spacing is 75μm-200μm. The length and width of columnar crystals of samples with different porosities were measured, and the average length of columnar crystals of all samples was calculated to be L = 0.64mm, and the average width was D = 0.51mm.

[0093] Step 3: According to the above D and L, set a = 0.3mm, b = 0.3mm, c = 0.6mm, f1 = 0.4mm, f2 = 0.5mm, f3 = 0.2mm, the target porosity of the porous structure is 12%, and construct a 10×10×10mm 3 3D model of the lattice structure with a constant powder layer thickness of 25 μm.

[0094] Step 4: Slice and layer the model in two dimensions, import the model slice layer file into the additive manufacturing software, and generate the slice scanning path. The mixed powder is formed by electron beam selective melting forming technology, and the scanning line spacing of the mixed powder preheating scan is set to 1.0 mm, and the scanning speed is (1.0-3.5)×10 4 mm / s, the scanning current is 25A, the electron beam deflection speed is 150mm / s-350mm / s, and the electron beam scanning line spacing is 75μm-200μm.

[0095] Step 5: Set the laser shock action path to impact the node and column area, and not impact the rest of the area, where the laser wavelength is 1064nm, the pulse width is 9ns, the laser energy is 2J-6J, and the spot diameter is 1mm. The laser shock is performed once after every three layers of material addition.

[0096] Step 6: Start the manufacturing of porous alloy components according to the preset parameters and paths. After the current layer is added, determine whether there is an impact area that needs interlayer laser shock according to the slice file. If laser shock is required, shock the node and cross column area once; if laser shock is not required, continue to add material to the next model layer.

[0097] Step 7: The manufactured component is subjected to thermomagnetic mechanical training, cycling between the martensite and austenite states in a rotating magnetic field of 0.97 T for 15 cycles.

[0098] Step 8: End.

[0099] <Comparative Example 1>

[0100] The same as Example 1, except that a conventional bcc porous structure is adopted and the interlayer laser shock technology is not used in the preparation process, and the other conditions remain unchanged.

[0101] <Comparative Example 2>

[0102] The same as the second embodiment, except that a conventional bcc porous structure is adopted and the interlayer laser shock technology is not used in the preparation process, and the other conditions remain unchanged.

[0103] According to the methods of Example 1 and Example 2, Comparative Example 1 and Comparative Example 2, Ni-Mn-Ga porous structure alloy components were prepared, and their porosity, grain morphology, maximum wide surface size of columnar crystals and shape memory effect were tested at room temperature. The test results are shown in Table 3:

[0104] Table 3

[0105]

[0106] It can be seen from Table 3 that the shape memory alloys prepared in all embodiments and comparative examples have controllable porosity; the shape memory alloys obtained by the preparation methods of Examples 1 and 2 have more beneficial bamboo-shaped grains than the shape memory alloys prepared in Comparative Examples 1 and 2, and have larger columnar crystal grain sizes when the porosity is similar, which is beneficial to improving the shape memory effect; the shape memory alloys obtained by the preparation methods of Examples 1 and 2 have significantly increased MFIS (magnetic induced strain) than the shape memory alloys prepared in Comparative Examples 1 and 2.

[0107] It should be noted that the serial numbers of the above-mentioned embodiments of the present application are only for description and do not represent the advantages or disadvantages of the embodiments.

[0108] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a composite ferromagnetic shape memory alloy porous structure, It is characterized in that The following steps are involved: Step 1: preparing ferromagnetic shape memory alloy powder; Step 2: using the configured ferromagnetic shape memory alloy powder to manufacture an initial body-centered cubic porous structure sample, and measuring and obtaining the average grain length and average grain width of columnar crystals of the initial body-centered cubic porous structure sample; Step 3: Construct a three-dimensional porous structure model based on the measured average grain length and average grain width of the columnar crystals; Step 4: Using a laser shock-laser additive manufacturing method to perform composite additive manufacturing on the imported three-dimensional porous structure model to obtain a component; Step 5: Perform thermal magnetic mechanical training on the component to obtain a composite ferromagnetic shape memory alloy porous structure device.

2. The method for preparing the composite ferromagnetic shape memory alloy porous structure according to claim 1, It is characterized in that In step 1, the ferromagnetic shape memory alloy selected is Ni-Mn-Ga alloy, and the ratio of each element in the ferromagnetic shape memory alloy powder is: Ni is 49wt%-51wt%, Mn is 28wt%-32wt%, and Ga is 19wt%-21wt%.

3. The method for preparing the composite ferromagnetic shape memory alloy porous structure as claimed in claim 1, It is characterized in that In the step 2, the porosity of the initial body-centered cubic porous structure sample is 10%-60%.

4. The method for preparing the composite ferromagnetic shape memory alloy porous structure according to claim 1, It is characterized in that In the step 2, the configured ferromagnetic shape memory alloy powder is used to manufacture an initial body-centered cubic porous structure sample by using laser selective melting technology.

5. The method for preparing the composite ferromagnetic shape memory alloy porous structure as claimed in claim 4, It is characterized in that In the laser selective melting technology, the laser power is 60W-100W, the scanning speed is 250mm / s-650mm / s, and the scanning interval is 50μm-100μm.

6. The method for preparing the composite ferromagnetic shape memory alloy porous structure as claimed in claim 1, It is characterized in that In the step 2, a conventional cubic porous structure sample is manufactured by using electron beam selective melting technology, direct laser forming technology, or arc additive manufacturing technology.

7. The method for preparing the composite ferromagnetic shape memory alloy porous structure as claimed in claim 6, It is characterized in that The step 3 specifically comprises the following steps: According to the measured average grain length L and average grain width D of the columnar crystals, the parameter setting constraints of a single lattice of the following three-dimensional porous structure model are constructed: c = (0.90-0.99) L; and f 1 、f 2 Both are smaller than D or f 1 f 2 <D 2 ;and, ab <f 1 f 2 ;and, f 3 =(0.10~0.45)c; Where a, b, and c are the lengths of the x-, y-, and z-directions of the pillars in a single lattice, respectively. 1 、f 2 、f 3 They are the x-axis pillar width, y-axis pillar width, and z-axis pillar width, respectively. L is the average grain length, and D is the average grain width. The three-dimensional porous structure model is set by setting constraint conditions based on the parameters of a single lattice of the constructed three-dimensional porous structure model.

8. The method for preparing the composite ferromagnetic shape memory alloy porous structure as claimed in claim 1, It is characterized in that The step 4 specifically comprises the following steps: Perform two-dimensional slicing and layering on the constructed three-dimensional porous structure model to obtain a model slicing and layering file; Import the model slice layering file and generate the slice scanning path; According to the model slicing and layering file, the imported three-dimensional porous structure model is processed layer by layer by composite additive manufacturing using a preparation method that alternates additive manufacturing and interlayer laser shock until the entire component is completed.

9. The method for preparing the composite ferromagnetic shape memory alloy porous structure as claimed in claim 8, It is characterized in that The method of performing composite additive manufacturing layer by layer on the imported three-dimensional porous structure model according to the model slice layer file by using an additive manufacturing and interlayer laser shock alternate preparation method until the entire component is completed specifically includes the following steps: Perform additive processing on the first layer of two-dimensional slices and layers of the imported three-dimensional porous structure model to obtain the required working conditions of laser shock for the current layer of two-dimensional slices and layers; If laser shock is required, the layer is laser shocked; If laser shock is not required, laser shock is not performed and the additive processing is continued on the next model layer; The above steps are repeated until the composite additive manufacturing processing of all two-dimensional slices and layers of the imported three-dimensional porous structure model is completed to obtain a component.

10. The method for preparing the composite ferromagnetic shape memory alloy porous structure according to claim 1, It is characterized in that The manufactured component is cycled between the martensite and austenite states under a rotating magnetic field, and the component is subjected to thermomagnetic mechanical training and cycled between the martensite and austenite states under a rotating magnetic field.