Method for improving steel surface wettability by using femtosecond laser surface texture

The textured treatment of the steel surface through femtosecond laser processing system solves the problem of insufficient wettability on the steel surface, significantly improves the bonding strength of the welded joints, and improves production efficiency.

CN118926705APending Publication Date: 2024-11-12SHANGHAI UNIV OF ENG SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411037461.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing welding methods cannot effectively improve the wettability of the steel surface, resulting in insufficient bonding strength of the aluminum-steel welded joints and affecting the welding quality.

Method used

The surface of steel material is mechanically polished, cleaned and etched by femtosecond laser processing system. By adjusting the parameters such as laser pulse frequency, pulse width, scanning speed and power, the textured surface texture is formed to improve the wettability of the steel surface.

Benefits of technology

It significantly improves the wettability of the steel surface, enhances the bonding strength of the welded joints, and prevents material oxidation in a closed argon environment, improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926705A_ABST
    Figure CN118926705A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving steel surface wettability through femtosecond laser surface texture. The method comprises the following steps that the surface of a steel material is mechanically ground and polished; cleaning with an acetone solution and ultrasonic waves; placing the cleaned steel material in a metal container; a femtosecond laser machining system is adopted for machining the steel material; and the surface of the machined steel material is cleaned. The method has the beneficial effects that according to the technical scheme, a femtosecond laser processing system is utilized, the surface of a steel material is etched according to a preset track by changing parameters such as pulse frequency, pulse width, scanning speed and power, the steel surface can be flexibly processed, and a surface texture with certain texturing is obtained; according to the technical scheme, machining is conducted in the closed inert gas, material oxidation in the machining process can be prevented, compared with the steel material surface not subjected to laser etching, the wettability of the steel surface subjected to laser etching is remarkably improved, the method is high in machining speed, and the production efficiency is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel surface treatment, in particular to a method for improving steel surface wettability by utilizing femtosecond laser surface texturing. Background Art

[0002] Aluminum alloy has excellent properties such as low density, good corrosion resistance, high electrical conductivity and thermal conductivity. Using aluminum alloy to replace steel can greatly reduce the quality of welded structures. Steel has good weldability and mechanical properties. Aluminum-steel welded structures have been widely used in automobile and shipbuilding industries. The melting point of aluminum is 660℃, which is 700-900℃ lower than that of steel. During welding, aluminum with a low melting point melts first, while steel is still not melted. Due to the large difference in density between aluminum and steel, the aluminum in the molten pool will float on the steel, which will cause uneven weld composition after cooling; the linear expansion coefficient between aluminum and steel is quite different, which will cause large residual stress in the weld joint and weld cracks.

[0003] In order to achieve a reliable connection between aluminum and steel, it is necessary to overcome the obstruction of the oxide film on the surface of aluminum and aluminum alloys to the connection, and to prevent or reduce the generation of brittle intermetallic compounds at the interface between aluminum alloy and steel. The existing welding methods are: pressure welding, brazing, and brazing. Among the three aluminum-steel dissimilar material welding methods, pressure welding and brazing process methods can achieve the connection between aluminum and steel.

[0004] At present, aluminum-steel dissimilar metal fusion-brazing welding has been widely used in the fields of automobile, aerospace and rail transportation. The wettability of brazing filler metal and molten aluminum alloy on the steel surface directly affects the bonding strength of the joint interface. The existing methods cannot improve the wettability of the steel surface, which seriously affects the bonding strength of the joint interface. Therefore, a method using femtosecond laser surface texturing to improve the wettability of the steel surface is designed. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems and to design a method for improving the wettability of steel surface by using femtosecond laser surface texturing.

[0006] To achieve the above object, the technical solution of the present invention is a method for improving the wettability of steel surface by using femtosecond laser surface texturing, comprising the following steps:

[0007] Step 1: Mechanically grind and polish the surface of the steel material;

[0008] Step 2: Clean with acetone solution and ultrasonic wave;

[0009] Step 3: Place the cleaned steel material in a metal container;

[0010] Step 4: Process the steel material using a femtosecond laser processing system;

[0011] Step 5: Clean the surface of the processed steel material.

[0012] As a further description of the technical solution, in step three, the metal container has a glass window.

[0013] As a further description of the technical solution, in step 4, the femtosecond laser processing system includes a laser, an attenuator, a reflector, a scanning galvanometer, an objective lens, a workpiece, and a metal container.

[0014] As a further description of the technical solution, the reflector and the attenuator are arranged at an angle of 60°.

[0015] As a further description of the technical solution, the reflector, the scanning galvanometer, the objective lens, and the workpiece are in the same vertical plane.

[0016] As a further description of the technical solution, the workpiece is placed in a closed metal container filled with argon atmosphere.

[0017] As a further description of the technical solution, in step 4, the parameters of the femtosecond laser processing system are as follows: laser pulse width 50-500fs, pulse frequency 10-28KHz, wavelength 1064nm, laser power 1-50W, spot diameter 20-60μm.

[0018] As a further description of the technical solution, the femtosecond laser processing system is started to scan the laser on the surface of the steel material at a certain speed, the scanning speed is 150-500mm / s, and finally a textured surface of a certain shape is obtained on the surface, the etching depth is 10-100μm, the etching spacing is 50-500μm, and the etching width is 15-50μm.

[0019] Its beneficial effect lies in that the technical solution utilizes a femtosecond laser processing system to perform etching on the surface of the steel material along a predetermined trajectory by changing parameters such as pulse frequency, pulse width, scanning speed, and power, and can flexibly process the steel surface to obtain a certain textured surface structure. The technical solution is processed in a closed inert gas to prevent oxidation of the material during the processing. Compared with the surface of the steel material that has not been laser-etched, the wettability of the steel surface that has been laser-etched is significantly improved. This method has a fast processing speed and effectively improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a schematic diagram of a femtosecond laser processing system of the present invention;

[0021] FIG. 2( a ) is a scanning path diagram of Example 1 of the present invention; FIG. 2( b ) and FIG. 2( c ) are circular surface texture diagrams of Example 1 of the present invention;

[0022] FIG. 3( a ) is a scanning path diagram of Example 2 of the present invention; FIG. 3( b ) and FIG. 3( c ) are surface texture diagrams of surface parallel lines of Example 2 of the present invention;

[0023] FIG. 4( a ) is a scanning path diagram of Example 3 of the present invention; FIG. 4( b ) and FIG. 4( c ) are surface spiral line surface texture diagrams of Example 3 of the present invention. DETAILED DESCRIPTION

[0024] First of all, the original intention of the design of the present invention is explained. At present, aluminum-steel dissimilar metal fusion-brazing welding has been widely used in the fields of automobiles, aerospace and rail transportation. The wettability of the brazing material and the molten aluminum alloy on the steel surface directly affects the bonding strength of the joint interface. The existing methods cannot improve the wettability of the steel surface, which seriously affects the bonding strength of the joint interface. Therefore, the present invention designs a method for improving the wettability of the steel surface using femtosecond laser surface texturing.

[0025] The present invention will be described in detail below in conjunction with the accompanying drawings. Figure 1 As shown, a method for improving the wettability of a steel surface by using femtosecond laser surface texturing comprises the following steps:

[0026] Step 1: Mechanically grind and polish the surface of the steel material;

[0027] Step 2: Clean with acetone solution and ultrasonic wave;

[0028] Step 3: placing the cleaned steel material in a metal container; in step 3, the metal container has a glass window;

[0029] Step 4: Use a femtosecond laser processing system to process the steel material; in the step 4, the femtosecond laser processing system includes a laser, an attenuator, a reflector, a scanning galvanometer, an objective lens, a workpiece, and a metal container, and the reflector is set at an angle of 60° to the attenuator; the reflector and the scanning galvanometer, the objective lens, and the workpiece are in the same vertical plane, and the workpiece is placed in a closed metal container filled with argon atmosphere.

[0030] In the step 4, the parameters of the femtosecond laser processing system are as follows: laser pulse width 50-500fs, pulse frequency 10-28KHz, wavelength 1064nm, laser power 1-50W, spot diameter 20-60μm; start the femtosecond laser processing system, make the laser scan the surface of the steel material at a certain speed, the scanning speed is 150-500mm / s, and finally a textured surface of a certain shape is obtained on the surface, the etching depth is 10-100μm, the etching spacing is 50-500μm, and the etching width is 15-50μm.

[0031] The laser emitted by the femtosecond laser transmitter is regulated by the attenuator to obtain the appropriate laser energy, and then the direction of the light path is changed under the action of the reflector. Through the action of the scanning galvanometer and the objective lens, the surface of the aluminum alloy plate is etched in a certain pre-track to obtain a textured surface of a certain shape to improve the wettability of the steel surface.

[0032] Step 5: Clean the surface of the processed steel material.

[0033] The following will be described in detail with reference to the embodiments:

[0034] Example 1

[0035] (1) Take a 1.5 mm thick DP980 steel sheet, mechanically grind and polish the surface of the material to a roughness of Ra = 12.5, and clean it with acetone solution and ultrasonic wave;

[0036] (2) Place the sample in Figure 1 The femtosecond laser processing system shown is placed inside a metal container to provide an inert gas environment to prevent oxidation of the metal surface during processing.

[0037] (3) Set the scanning processing area size to 40 mm × 40 mm, the laser power to 30 W, the scanning speed to 300 mm / s, the frequency to 20 kHz, the scanning spacing to 150 μm, and the scanning path as shown in Figure 2(a). Start the laser processing system to start etching on the steel surface.

[0038] (4): After processing, the workpiece is taken out and wiped clean with anhydrous ethanol to obtain a circular surface texture pattern with a diameter of 45μm, a depth of 15μm, and a spacing of 150μm, as shown in Figures 2(b) and 2(c). Compared with the steel without surface texture, the wettability is significantly improved.

[0039] Example 2

[0040] (1) Take a 1.5 mm thick 316L stainless steel sheet, mechanically grind and polish the surface of the material to a roughness of Ra = 12.5, and clean it with acetone solution and ultrasonic wave.

[0041] (2) Place the sample in Figure 1 The laser processing system shown is inside a metal container to provide an inert gas environment to prevent oxidation of the metal surface during processing.

[0042] (3) Set the scanning processing area size to 40 mm × 40 mm, the laser power to 30 W, the scanning speed to 250 mm / s, the frequency to 18 kHz, the scanning spacing to 120 μm, and the scanning path as shown in Figure 3(a). Start the laser processing system to start etching on the steel surface.

[0043] (4): After processing, the workpiece was taken out and cleaned with anhydrous ethanol to obtain a parallel line texture pattern with a width of 50 μm, a depth of 20 μm, and a spacing of 120 μm, as shown in Figures 3(b) and 3(c). Compared with the steel without surface texture, the wettability is significantly improved.

[0044] Example 3

[0045] (1) Take 2 mm thick DC04 low carbon steel, mechanically grind and polish the surface of the material to a roughness of Ra = 12.5, and clean it with acetone solution and ultrasonic wave.

[0046] (2) Place the sample in Figure 1 The laser processing system shown is inside a metal container to provide an inert gas environment to prevent oxidation of the metal surface during processing.

[0047] (3) Set the scanning processing area size to a circular area of ​​40 mm, the laser power to 15 W, the scanning speed to 200 mm / s, the frequency to 18 kHz, and the processing path to be spiral with a pitch of 80 μm. The scanning path is shown in Figure 4(a). Start the laser processing system to start etching on the steel surface.

[0048] (4): After processing, the workpiece was taken out and wiped clean with anhydrous ethanol to obtain a spiral texture pattern with a width of 30 μm, a depth of 10 μm, and a spacing of 80 μm, as shown in Figures 4(b) and 4(c). Compared with the steel without surface texture, the wettability was significantly improved.

[0049] This technical solution utilizes a femtosecond laser processing system to perform etching on the surface of a steel material along a predetermined trajectory by changing parameters such as pulse frequency, pulse width, scanning speed, and power. The steel surface can be flexibly processed to obtain a certain textured surface structure. This technical solution is processed in a closed inert gas to prevent oxidation of the material during the processing. Compared with the surface of the steel material that has not been laser-etched, the wettability of the steel surface that has been laser-etched is significantly improved. This method has a fast processing speed and effectively improves production efficiency.

[0050] The above technical solutions only reflect the preferred technical solutions of the technical solutions of the present invention. Some changes that may be made to certain parts thereof by technicians in this technical field all reflect the principles of the present invention and fall within the protection scope of the present invention.

Claims

1. A method for improving the wettability of a steel surface by using femtosecond laser surface texturing, characterized in that: The following steps are involved: Step 1: Mechanically grind and polish the surface of the steel material; Step 2: Clean with acetone solution and ultrasonic wave; Step 3: Place the cleaned steel material in a metal container; Step 4: Process the steel material using a femtosecond laser processing system; Step 5: Clean the surface of the processed steel material.

2. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 1, characterized in that: In step three, the metal container has a glass window.

3. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 1, characterized in that: In the step 4, the femtosecond laser processing system includes a laser, an attenuator, a reflector, a scanning galvanometer, an objective lens, a workpiece, and a metal container.

4. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 3, characterized in that: The reflector and the attenuator are arranged at an angle of 60°.

5. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 3, characterized in that: The reflector, the scanning galvanometer, the objective lens and the workpiece are located in the same vertical plane.

6. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 1, characterized in that: The workpiece is placed in a sealed metal container filled with argon atmosphere.

7. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 1, characterized in that: In the step 4, the parameters of the femtosecond laser processing system are as follows: laser pulse width 50-500fs, pulse frequency 10-28KHz, wavelength 1064nm, laser power 1-50W, spot diameter 20-60μm.

8. The method for improving the wettability of steel surface by using femtosecond laser surface texturing according to claim 7, characterized in that: Start the femtosecond laser processing system to scan the laser on the surface of the steel material at a certain speed of 150-500mm / s, and finally obtain a textured surface of a certain shape on the surface, with an etching depth of 10-100μm, an etching spacing of 50-500μm, and an etching width of 15-50μm.

Citation Information

Cited By

  • Method for preparing antireflection surface on metal copper surface

    CN120460884A