Steel material for high-interface-bonding-force metal connector, metal connector and manufacturing method
By setting up several recessed structures and special transition layers on the surface of the steel material, the problem of insufficient interface bonding in steel-aluminum heterogeneous metal connection is solved, the crack resistance of the interface layer is improved, and the steel-aluminum heterogeneous metal with high interface bonding is formed Connecting the joints avoids interface failure and fracture and increases the spread area of weld metal.
Patent Information
- Application Number
- CN202411428096.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-14
AI Technical Summary
In steel and aluminum different metal connections, the prior art has insufficient interface crack resistance and binding force, which leads to the joint prone to interface failure and fracture.
Several recessed structures are set up on the surface of the steel material to form a non-planar three-dimensional structure, combining special transition layers and plating layers to improve the spreadability of the liquid weld metal and the crack-resistance of the interface layer, and enhance the bonding force of the connection interface.
Improve the spreadability of liquid weld metal on the surface of steel material and the crack-resistant expansion ability of the interface layer, forming a steel-aluminum heterogeneous metal joint with high interface bonding force, avoiding interface failure and fracture, and enhancing the weld metal The spread area is about 40%.
Smart Images

Figure CN118926765A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of steel-aluminum dissimilar metal connection, and specifically relates to a steel material for a metal connection joint with high interface bonding strength, a metal connection joint and a manufacturing method. Background Art
[0002] At present, there are two main directions for lightweight strategies in vehicle body structure design. One is to use advanced high-strength steel materials to achieve thinning and weight reduction of structural parts, and the other is to use lightweight materials instead of steel materials to achieve weight reduction. Aluminum alloy has a low density, about 1 / 3 of that of steel materials, high specific strength and specific stiffness, and can reduce the weight of vehicle body parts with the same performance by more than 30%. It is one of the most promising lightweight materials in vehicle body lightweight design. Although aluminum alloy has more potential than steel materials in terms of vehicle body lightweighting, the collision performance of aluminum alloy in some key safety parts of the vehicle body cannot be compared with advanced high-strength steel. Therefore, from the dual perspectives of lightweight and safety, steel-aluminum hybrid vehicles will become the mainstream vehicle body lightweight design solution in the future.
[0003] The bottleneck problem that needs to be solved in the steel-aluminum hybrid body solution is the connection problem between steel and aluminum. The inherent disparity in physical properties between steel and aluminum alloys determines that the two cannot be connected together using traditional fusion welding technology, and only fusion brazing technology can be used to connect steel and aluminum alloys. During the steel-aluminum fusion brazing process, under the action of the heat source, the steel does not melt, and the aluminum alloy and filler metal are melted and mixed to form liquid weld metal, which spreads a certain width on the surface of the steel plate. In the subsequent cooling and solidification process, an intermetallic compound layer with a certain thickness is formed on the interface between the liquid weld metal and the steel, thereby realizing the metallurgical connection of steel and aluminum dissimilar metals.
[0004] For steel-aluminum dissimilar metal fusion brazing joints, the interfacial bonding strength between steel and weld metal is the core factor that determines the performance of steel-aluminum dissimilar metal fusion brazing joints. The effective spreading width of the liquid weld metal on the steel surface directly determines the interfacial bonding strength between steel and weld metal. Regarding steel-aluminum dissimilar metal connections, although some improvement methods have been proposed in recent years, there is still a large gap between the performance of the joint and the aluminum alloy parent material. Under load conditions, the steel-aluminum joint will fail and fracture due to insufficient interfacial bonding strength. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the problems of the prior art steel-aluminum joint interface, such as insufficient crack propagation resistance and insufficient interface bonding strength, and easy interface failure and fracture, so as to provide a steel material, a metal connection joint and a manufacturing method for a high interface bonding strength metal connection joint.
[0006] To this end, the present invention provides the following technical solutions.
[0007] In a first aspect, the present invention provides a steel material for a metal connection joint with high interface bonding strength, wherein at least a plurality of recessed structures are arranged on the surface of the steel material connected to the aluminum alloy, and the total area of the projections of the plurality of recessed structures on the surface of the steel material is denoted as S. 1 The area of the region enclosed by the projection is recorded as S 0 The maximum depth of the several concave structures is denoted as D 0 The projected area of a single depression on the surface of the steel material is recorded as S 2 , the width of the area enclosed by the projection is recorded as W 0 ; said W 0 ≥3mm; D 0 :0.05mm≤D 0 ≤1.0mm; S 2 : 0.25D 0 2 ≤S 2 ≤25D 0 2 ; The S 1 and S 0 Satisfy relation 1; Relationship 1.
[0008] As an example, the S 1 and S 0 The ratio is 0.05, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.95 or any two numerical ranges. 0 Any value such as 3mm, 6mm, 9mm, 12mm, 15mm, 18mm, 21mm, 24mm, 27mm, etc. 0 Any value such as 0.05mm, 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1.0mm, etc. The projection area of a single concave structure on the surface of the steel material meets 0.25D 0 2 ≤S 2 ≤25D 0 2 , no specific requirements are made.
[0009] In an optional embodiment, the shape of the projection of the recessed structure on the surface of the steel material is an arbitrary shape. Preferably, the shape of the projection of the recessed structure on the surface of the steel material includes at least one of a regular shape and an irregular shape; the shape of the projection of the recessed structure on the surface of the steel material includes but is not limited to at least one of a circle, a triangle, a polygon and an irregular shape.
[0010] In an optional embodiment, from outside to inside, the surface of the steel material includes a non-oxidized layer and a transition layer; Preferably, the oxygen content in the grain boundary of the transition layer is 5-47wt%. As an example, the oxygen content in the grain boundary of the transition layer is 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 47wt% or any two numerical ranges.
[0011] In an optional embodiment, the thickness of the transition layer T 1 0.1-15μm; Preferably, the thickness of the steel material is not greater than 8 mm; Preferably, the tensile strength of the steel material at room temperature is not less than 200 MPa.
[0012] In an optional embodiment, a coating is provided on the surface of the steel material; Preferably, the material of the coating is at least one of a zinc-based material, an aluminum-based material and a nickel-based material; Preferably, the coating is made of zinc-based material.
[0013] A second aspect of the present invention provides a metal connection joint, comprising a steel material, an aluminum alloy and a weld; the steel material comes from the above-mentioned steel material.
[0014] In an optional embodiment, the weld includes an intermetallic compound layer, and the thickness T of the intermetallic compound layer is IMC Not more than 30μm; Preferably, the thickness T of the intermetallic compound layer is IMC :T IMC ≥2μm.
[0015] In an optional embodiment, the aluminum alloy is 5XXX series or 6XXX series; it should be noted that 5XXX series and 6XXX series refer to the types of aluminum alloys; Preferably, the thickness of the aluminum alloy is not greater than 8 mm.
[0016] A third aspect of the present invention provides a method for manufacturing a metal connecting joint, which uses the above-mentioned steel material; filler material and aluminum alloy are melted to form liquid metal, and the liquid metal spreads on the surface of the steel material and solidifies.
[0017] In an optional embodiment, the spreading width L 0 No greater than W 0 ; Preferably, the spreading width L 0 Not less than 1mm; Preferably, the spreading width L 0 :L 0 ≤15mm.
[0018] The spreading width refers to the distance that the liquid metal spreads on the surface of the steel material perpendicular to the welding direction.
[0019] The technical solution of the present invention has the following advantages: 1. The steel material for high interface bonding strength metal connection joint provided by the present invention has a plurality of recessed structures at least in the surface area of the steel material connected with the aluminum alloy, and the total area of the projections of the plurality of recessed structures on the surface of the steel material is denoted as S. 1 The area of the region enclosed by the projection is recorded as S 0 The maximum depth of the several concave structures is denoted as D 0 The projected area of a single depression on the surface of the steel material is recorded as S 2 , the width of the area enclosed by the projection is recorded as W 0 ; said W 0 ≥3mm; D 0 :0.05mm≤D 0 ≤1.0mm; S 2 : 0.25D 0 2 ≤S 2 ≤25D 0 2 ; The S 1 and S 0 Satisfies the relationship 1. The application of the steel material to steel-aluminum dissimilar metal joints can improve the spreadability of the liquid weld metal on the surface of the steel material, enhance the ability of the interface layer to resist crack propagation, and improve the bonding strength at the connection interface, and the interface connection will not have problems such as fracture failure. The steel material can be connected to the aluminum alloy by generating intermetallic compounds with the weld metal to form a steel-aluminum dissimilar metal connection joint with high interface bonding strength. Under tensile shear loads, the joint will preferentially fail at the aluminum alloy parent material fracture rather than at the interface. The surface of the steel material is provided with a number of recessed structures. This non-planar three-dimensional structure increases the spreading width and area of the liquid weld metal on the surface of the steel material, improves the ability of the interface layer to resist crack propagation, and enhances the spreadability of the liquid weld metal. Finally, a steel-aluminum dissimilar metal connection joint with high interface bonding strength is obtained, solving the problem of interface failure of the steel-aluminum joint.
[0020] Furthermore, the steel material of the present invention satisfies W 0 Not less than 3mm, 0.05mm≤D 0 ≤1.0mm, 0.25D 0 2 ≤S 2 ≤25D0 2 , and S 1 and S 0 The ratio of meets 0.05-0.95, which can greatly increase the spreading area of the liquid weld metal. Under the same spreading width, the special structure of the steel material of the present invention increases the spreading area by about 40% compared with the flat structure. In addition, the concave structure of the special structure can also ensure that the spreading width L of the liquid weld metal is 0 .
[0021] 2. The steel material for high interface bonding strength metal connection joints provided by the present invention is provided with a special transition layer, which can improve the spreading performance of the weld metal on the surface of the steel material, and help the liquid weld metal to form an intermetallic compound layer with uniform thickness, complete structure and no crack defects on the surface of the steel material. The surface of the steel material is provided with an oxygen-free layer and a transition layer, and the oxygen-free layer can reduce the interfacial tension between the weld metal and the surface of the steel material, and significantly improve the spreading ability of the liquid weld metal on the surface of the steel material; the present invention is the first to apply a steel material with a transition layer having a certain grain boundary oxygen content on the secondary surface to a metal connection joint, and can prepare an intermetallic compound layer with more uniform thickness and higher structural consistency, which can further effectively avoid the formation of microcracks in the intermetallic compound layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 is a schematic diagram of the area formed by enclosing the projection in the present invention; Figure 2 is another schematic diagram of the area formed by enclosing the projection in the present invention; Figure 3 This is a schematic diagram of the enclosed projection area of the steel material in Example 1 of the present invention; Figure 4 is a schematic structural diagram of a metal joint according to Embodiment 1 of the present invention; Figure 5 This is a schematic diagram of the enclosed projection area of the steel material in Example 9 of the present invention; Figure 6 This is a schematic diagram of the enclosed projection area of the steel material in Example 10 of the present invention; Figure 7 This is a schematic diagram of the fracture interface of a metal joint in a comparative example of the present invention; Reference numerals: 1-first line; 2-second line; 3-third line; 4-fourth line; 5-fifth line; 6-sixth line; 7-seventh line; 8-eighth line; 9-steel material; 10-weld; 11-aluminum alloy. DETAILED DESCRIPTION
[0024] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0025] In the prior art, when aluminum alloy is overlapped on the surface of steel material for welding to form a steel-aluminum dissimilar connection joint, the interface crack propagation resistance and bonding strength are insufficient, and interface failure and fracture are prone to occur. In order to solve the problems existing in the prior art, the present invention provides a steel material, which is applied to the metal connection joint, and the interface joint has good interface bonding strength and crack propagation resistance. The solution provided by the present invention is as follows.
[0026] The present invention provides a steel material for a metal connection joint with high interface bonding strength. The surface of the steel material is pre-processed by rolling, machining or laser processing to form a non-planar three-dimensional structure on the surface. A plurality of recessed structures are arranged on the surface of the steel material connected to the aluminum alloy. The non-planar three-dimensional structure is a total area of the projections of the plurality of recessed structures on the surface of the steel material is recorded as S. 1 The area of the region enclosed by the projection is recorded as S 0 The maximum depth of the several concave structures is denoted as D 0 , the width of the area enclosed by the projection is recorded as W 0 ; said W 0 ≥3mm; D 0 :0.05mm≤D 0 ≤1.0mm; S 2 : 0.25D 0 2 ≤S 2 ≤25D 0 2 ; The S 1 and S 0 Satisfy relation 1; Relationship 1.
[0027] Among them, a plurality of concave structures are arranged regularly or irregularly on the surface of the steel material, a plurality of concave structures can be the same or different, the depths of a plurality of concave structures can be the same or different, the shape of their projection on the surface of the steel material is an arbitrary shape, and the shape of the projection of the concave structure on the surface of the steel material includes at least one of a regular shape and an irregular shape, including but not limited to at least one of a circle, a triangle, a polygon and an irregular shape. The shape of the concave structure can be any non-planar three-dimensional structure such as a hemisphere, an inverted pyramid, an inverted quadrangular pyramid, etc. The projection of a single concave structure on the surface of the steel material satisfies 0.25D 0 2 ≤S 2 ≤25D 0 2 That is, there is no specific restriction on the projection area of a single recessed structure, and the projection areas of different recessed structures may be the same or different.
[0028] It should be noted that other areas on the surface of the steel material may be provided with a number of recessed structures or may be planar structures, depending on demand and cost. The projection refers to the projection of the recessed structure on the surface of the steel material along the thickness direction of the steel material. The area enclosed by the projection refers to a closed area formed by the outermost points of the projection located at the edge of the area (also called edge points) enclosed in sequence by straight lines and / or the reverse extension of the straight lines; the area is preferably a regular shape, such as a polygon such as a triangle, rectangle, pentagon, hexagon, etc., refer to Figure 1 and Figure 2 , not limited to Figure 1 and Figure 2 Shapes listed.
[0029] by Figure 1 For example, the first line 1 and the second line 2 are formed by the straight lines connecting the two different tangent points of the circle and the points outside the two quadrilaterals and their reverse extension lines, and the third line 3 is formed by the straight lines connecting the points outside the quadrilaterals and their reverse extension lines. The closed area formed by the first line 1, the second line 2 and the third line 3 is the area enclosed by the projection, and the area is recorded as S 0 .by Figure 2 For example, the fourth line 4 formed by the ellipse tangent point, the circle tangent point and the prism edge point, the fifth line 5 formed by the prism edge point, the sixth line 6 formed by the prism and the triangle edge point, the seventh line 7 formed by the edge points of two triangles, the eighth line 8 formed by the triangle edge point, the prism edge point and the ellipse tangent point, the fourth line 4, the fifth line 5, the sixth line 6, the seventh line 7 and the eighth line 8 form a closed area, which is the area enclosed by the projection, and the area is recorded as S 0 It will be appreciated that the area lines may overlap a certain edge of the projection; the area may not extend through the projection.
[0030] The width of the area enclosed by the projection refers to the average value of the minimum length and the maximum length of the area enclosed by the projection along the direction perpendicular to the welding direction. It can be understood that the minimum length includes the case of 0.
[0031] From the outside to the inside of the steel material, the surface of the steel material includes a non-oxidized layer and a transition layer; wherein the non-oxidized layer means that the surface of the steel material is not oxidized; the transition layer is located on the side of the non-oxidized layer away from the surface of the steel material, and the transition layer grain boundary contains a certain amount of oxygen, which exists in the form of oxides, and the oxidized elements are alloy elements in the steel matrix, such as iron, manganese, silicon, etc. It should be noted that the oxygen content in the transition layer grain boundary is obtained by testing according to methods known in the art, such as: X-ray energy spectrum (Energy-dispersive X-ray spectroscopy, EDS) micro-area composition analysis.
[0032] In the present invention, the tensile strength of the steel material at room temperature is not less than 200 MPa; the tensile strength of the steel material is tested by conventional testing methods in the art, such as GB / T 228-2010 Room temperature test method for tensile testing of metallic materials.
[0033] The present invention also provides a metal connecting joint, comprising a steel material, an aluminum alloy and a weld; the steel material comes from the above-mentioned steel material.
[0034] The steel and aluminum alloy joints are overlapped, and the aluminum alloy is overlapped on the surface of the steel material. The aluminum alloy and the filler material are melted by laser, electric arc, laser arc combination, etc. The aluminum alloy and the filler material form liquid weld metal and spread on the unmelted steel surface. The liquid weld metal has good spreadability on the surface of the above-mentioned special structural steel material, and after solidification, it generates intermetallic compounds, which are three-dimensional interface layers. Compared with the traditional plane structure interface layer, when the crack propagates in the three-dimensional interface layer with the same surface, this three-dimensional interface layer increases the crack propagation resistance in the interface layer and increases the crack propagation distance, so that the interface of the connection joint has excellent crack propagation resistance.
[0035] The filling material is a material known in the art, such as welding wire, metal powder, etc.
[0036] The process parameters of the laser, arc, laser arc composite and other methods are selected from the parameters known in the art to ensure that the aluminum alloy and the filling material can be melted, without strict requirements on the parameters, and different parameters do not affect the effect of the present invention.
[0037] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0038] Example 1 This embodiment provides a method for manufacturing a metal connection joint, comprising the following steps: (1) Low alloy high strength steel is selected as the steel material with a thickness of 1.4 mm. Several inverted triangular pyramid structures are prefabricated at the welding position of the steel material by roller pressing. Along the thickness direction of the steel material, the projection shape of the concave structure on the surface of the steel material is triangular and of the same size. The average value of the minimum width and maximum width of the area enclosed by these projections is W. 0 The area is 10 mm, and the area is recorded as S 0 The length of this area along the welding direction is recorded as W 1 , the enclosed schematic diagram of the projection area is shown in Figure 3 ,by Figure 3 As shown, S 0 =W 0 ×W 1 ; The maximum depth D of all recessed structures 0 0.3mm, maximum depth D 0 See the schematic diagram Figure 4 , Figure 4 9 is steel material, 10 is weld, and 11 is aluminum alloy; the projection area S of a single concave structure on the surface of the steel material 2 For 4D 0 2 The total projection area of all the concave structures on the steel surface is recorded as S 1 , the sum of the projected areas of all the recessed structures on the steel surface S 1 The area S of the region enclosed by all projections 0 The ratio is 0.5 (S 1 / S 0 ), steel transition layer thickness T 1 is 2.3 μm, and the oxygen content of the grain boundary in the transition layer is C O In this embodiment, the region is a closed region formed by connecting the outermost points of the projection located at the edge in sequence with straight lines and / or reverse extensions of adjacent straight lines.
[0039] Select 5XXX series aluminum alloy sheet with a thickness of 1.6 mm.
[0040] Commercial ER4043 aluminum-based welding wire is used as the filler material, and the diameter of the welding wire is 1.2 mm.
[0041] (2) Select laser as the heat source, the heat source moving speed is 600mm / min, and the heat input is 220J / mm; the filling rate of welding wire is 1500mm / min, and the welding wire and part of the aluminum alloy melt to form liquid weld metal spreading on the surface of the steel material, with a spreading width L 0and the width W of the area formed by the enclosed projection 0 See the schematic diagram of Figure 4 After solidification, a steel-aluminum dissimilar metal connection joint is obtained.
[0042] A scanning electron microscope is used to test the linear spreading width of the weld metal in the steel-aluminum dissimilar metal connection joint and the thickness of the intermetallic compound formed by the weld metal on the surface of the steel material.
[0043] Embodiment 2-8 Embodiment 2-8 provides a method for manufacturing a metal connection joint, which differs from Embodiment 1 in that the recess structure and parameters are different, the thickness and oxygen content of the transition layer are different, and the heat source during the preparation process is different.
[0044] The recessed structures and parameters, transition layer thickness and oxygen content, and heat sources during the preparation process of each embodiment are shown in Table 1-2.
[0045] Example 9 This embodiment provides a method for manufacturing a metal connection joint, comprising the following steps: (1) Low alloy high strength steel is selected as the steel material with a thickness of 1.6 mm. Laser processing is used to prefabricate inverted triangular pyramid, inverted quadrangular pyramid, and hemispherical concave structures at the welding position of the steel material. The concave structures of the same shape have the same size. Along the thickness direction of the steel material, the projection of the concave structure on the surface of the steel material is in the shape of a triangle, a quadrilateral, and a circle, with the proportion of 10%, 40%, and 50% respectively. The width W of the area enclosed by these projections is 0 is 12mm, and the area is denoted as S 0 , see the schematic diagram Figure 5 ; The maximum depth D of all the concave structures 0 The area of a single triangle is 4.6D. 0 2 , the single area of the projection as a quadrilateral is 7.6D 0 2 , the single area projected as a circle is 2.8D 0 2 The total projection area of all the concave structures on the steel surface is recorded as S 1 , the sum of the projected areas of all the recessed structures on the steel surface S 1 The area S of the region enclosed by all projections 0 The ratio is 0.3 (S 1 / S 0 ), steel transition layer thickness T 1 is 3.8μm, and the oxygen content of the grain boundary in the transition layer is C O is 25%.
[0046] Select 5XXX series aluminum alloy sheet with a thickness of 1.8 mm.
[0047] Commercial ER4043 welding wire is used as the filler material, and the diameter of the welding wire is 1.2 mm.
[0048] (2) The arc is selected as the heat source, the heat source movement rate is 25 mm / s, and the heat input is 1500 J / mm; the filling rate of the welding wire is 2300 mm / min, and a steel-aluminum dissimilar metal connection joint is obtained after solidification.
[0049] A scanning electron microscope is used to test the linear spreading width of the weld metal in the steel-aluminum dissimilar metal connection joint and the thickness of the intermetallic compound formed by the weld metal on the surface of the steel material.
[0050] Example 10 This embodiment provides a method for manufacturing a metal connection joint, comprising the following steps: (1) Low alloy high strength steel is selected as the steel material with a thickness of 1.0 mm. A hemispherical concave structure is prefabricated at the welding position of the steel material by machining. Along the thickness direction of the steel material, the projection of the concave structure on the surface of the steel material is circular, and the width W of the area enclosed by these projections is 0 is 8mm, and the area is denoted as S 0 , see the schematic diagram Figure 6 ; The maximum depth D of all recessed structures 0 The projected area of different concave structures is between 0.18 and 0.35 mm, but the projected area of a single concave structure is between 0.9 and 3.6 D. 0 2 The total projection area of all the concave structures on the steel surface is recorded as S 1 , the sum of the projected areas of all the recessed structures on the steel surface S 1 The area S of the region enclosed by all projections 0 The ratio is 0.7 (S 1 / S 0 ), steel transition layer thickness T 1 is 1.5μm, and the oxygen content of the grain boundary in the transition layer is C O In this embodiment, the area is a closed area formed by connecting the outermost tangent points of the circle located at the edge with straight lines or the reverse extension lines of adjacent straight lines, referring to Figure 6 .
[0051] Select 5XXX series aluminum alloy sheet with a thickness of 1.4 mm.
[0052] Commercial ER4047 welding wire is used as the filler material, and the diameter of the welding wire is 1.2 mm.
[0053] (2) Laser / arc was selected as the heat source, the heat source moving rate was 500 mm / s, and the heat input was 1100 J / mm; the filling rate of the welding wire was 1800 mm / min, and a steel-aluminum dissimilar metal connection joint was obtained after solidification.
[0054] A scanning electron microscope is used to test the linear spreading width of the weld metal in the steel-aluminum dissimilar metal connection joint and the thickness of the intermetallic compound formed by the weld metal on the surface of the steel material.
[0055] Comparative Example 1-2 Comparative Example 1-2 provides a method for manufacturing a metal connection joint, which is different from Example 1 in that the steel material surface is not subjected to a concave treatment and has a planar structure. The parameters of the manufacturing process are shown in Table 1-2.
[0056] Comparative Examples 3-5 Comparative Examples 3-5 provide a method for manufacturing a metal connection joint, which differs from Example 1 in that the parameters of the recessed structure are different. The recessed structures and parameters, transition layer thickness and oxygen content, and heat sources during the preparation process of each comparative example are shown in Table 1-2.
[0057] Table 1 Parameters of metal connection joints
[0058] Note: Unless otherwise specified, the projection shape and size are the same; the same heat source uses the same process parameters; “-” means that the parameter does not exist.
[0059] Table 2 Parameters of metal connection joints
[0060] Note: “-” means the parameter does not exist.
[0061] The performance of metal connection joints was tested according to GB / T 228-2010 Metal Material Tensile Test Room Temperature Test Method. The results are shown in Table 3.
[0062] Table 3 Performance of metal connection joints
[0063] Conclusion: According to the results in Table 3, the present invention provides a plurality of concave structures on the surface of the steel material, and the concave structures meet the requirements of W 0 Not less than 3mm, 0.05mm≤D 0 ≤1.0mm, 0.25D 0 2 ≤S 2 ≤25D 0 2 , and S 1 and S 0The ratio satisfies 0.05-0.95, forming a steel-aluminum dissimilar metal connection joint with high interface bonding strength. Under tensile shear load, the joint preferentially fails at the aluminum alloy base material rather than at the interface, thereby improving the ability of the interface layer to resist crack propagation and greatly increasing the spreading area of the liquid weld metal. Under the condition of the same spreading width, the special structure of the steel material of the present invention has a spreading area increased by about 40% compared with the plane structure.
[0064] From comparative examples 1-2, the recessed structure provided in the present invention can greatly improve the joint strength, will not break at the joint, and has significantly higher strength; Figure 7 This is the fractured sample of comparative example 1, indicating that the comparative example joint has poor performance and fracture occurs at the interface. 0 Not less than 3mm, 0.05mm≤D 0 ≤1.0mm, 0.25D 0 2 ≤S 2 ≤25D 0 2 , and S 1 and S 0 The ratio of satisfies 0.05-0.95, forming a steel-aluminum dissimilar metal connection joint with high interface bonding strength, which has great application value for dissimilar metal brazing. From comparative examples 1-5, although comparative examples 3-5 break at the interface between the weld metal and the steel material, the joint strength is still higher than that of the steel material without the recessed structure.
[0065] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A steel material for a metal connection joint with high interface bonding strength, characterized in that: At least a plurality of recessed structures are provided in the surface area of the steel material connected to the aluminum alloy, the total area of the projections of the plurality of recessed structures on the surface of the steel material is recorded as S1, the area of the area formed by the projections is recorded as S0, the maximum depth of the plurality of recessed structures is recorded as D0, the projection area of a single recess on the surface of the steel material is recorded as S2, and the width of the area formed by the projections is recorded as W0; W0 ≥ 3 mm; D0: 0.05 mm ≤ D0 ≤ 1.0 mm; S2: 0.25 D0 2 ≤S2≤25D0 2 ; S1 and S0 satisfy the relation 1; Relationship 1.
2. The steel material according to claim 1, characterized in that: The projection shape of the recessed structure on the surface of the steel material is any shape; The width of the area enclosed by the projection is the average of the minimum length and the maximum length of the area enclosed by the projection along the direction perpendicular to the welding direction.
3. The steel material according to claim 2, characterized in that: The projection shape of the concave structure on the surface of the steel material includes at least one of a regular shape and an irregular shape.
4. The steel material according to claim 2, characterized in that: The projection shape of the concave structure on the surface of the steel material includes at least one of a circular shape, a polygonal shape and an irregular shape.
5. The steel material according to claim 1 or 2, characterized in that: From the outside to the inside, the surface of the steel material includes a non-oxidized layer and a transition layer; The oxygen content in the grain boundaries of the transition layer is 5-47wt%.
6. The steel material according to claim 5, characterized in that: The thickness T1 of the transition layer is 0.1-15 μm; The thickness of the steel material is not more than 8mm; The tensile strength of the steel material at room temperature is not less than 200 MPa.
7. The steel material according to claim 1, characterized in that: A coating is provided on the surface of the steel material; The material of the coating is at least one of a zinc-based material, an aluminum-based material and a nickel-based material.
8. The steel material according to claim 7, characterized in that: The material of the coating is zinc-based material.
9. A metal connection joint, characterized in that: It comprises steel material, aluminum alloy and welding seam; the steel material is the steel material described in any one of claims 1-8.
10. The metal connection joint according to claim 9, characterized in that: The weld includes an intermetallic compound layer, the thickness of the intermetallic compound layer is T IMC Not more than 30μm; The thickness T of the intermetallic compound layer IMC :T IMC ≥2μm.
11. The metal connection joint according to claim 9 or 10, characterized in that: The aluminum alloy is 5XXX series or 6XXX series; The thickness of the aluminum alloy is not greater than 8 mm.
12. A method for manufacturing a metal connection joint, characterized in that: The steel material according to any one of claims 1 to 8 is used; the filler material and the aluminum alloy are melted to form liquid metal, and the liquid metal spreads on the surface of the steel material and solidifies.
13. The manufacturing method according to claim 12, characterized in that: The spreading width L0 is not greater than W0; The spreading width L0 is not less than 1 mm; The spreading width L0: L0≤15mm.
Citation Information
Patent Citations
Aluminum / steel laser welding method under action of Cu element-surface micro-texture composite regulation
CN111958113A
Laser-double TIG electric arc composite self-fluxing brazing method for aluminum alloy and stainless steel
CN113427132A
Low-heat-input laser brazing method for aluminum-steel dissimilar metal
CN114632987A
Metallic join partners` connecting method for manufacturing vehicle body, involves grouting two join partners, so that material of latter partner penetrates into recess of former partner to produce fixed connection between partners