Preparation method of spherical smelting flux

Through the air quenching granulation forming method, the problems of unsafe forming and poor fluidity of the smelting flux water quenching method are solved, uniform forming and stable feeding of spherical particles are achieved, and the quality and performance of the welding bead are improved.

CN118926766APending Publication Date: 2024-11-12WUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410969655.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing water quenching method of smelting flux has unsafe operation, irregular particle shape and poor fluidity, resulting in insufficient quality and mechanical properties of the weld beads, and it is easy to cause feeding blockage and pore defects.

Method used

Using the air-quenched granulation forming method, the flux melt is formed through the tundra and supersonic nozzle to form a high-pressure and high-speed jet, cut into atomized melt droplets and cooled in the atomization box, and the particles are separated by a spiral separator and collected directly. Spherical particles ensure flux fluidity and formability.

Benefits of technology

It improves the safety of production operations, the particles are not easy to powder, good fluidity, uniform flux feeding, and uniform molten pool coverage, avoids pore defects in the welding beads and ensures the formingability and mechanical properties of the welding beads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926766A_ABST
    Figure CN118926766A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a spherical smelting flux. The preparation method comprises the following steps: (1) uniformly stirring and mixing designed flux ingredients, and baking; (2) putting into a smelting furnace which is preheated to a high temperature; (3) the flux melt flows into a tundish through an outflow groove of the smelting furnace, a cut-off dam is arranged, and flux melt jet flow is formed; (4) melt jet flow air quenching granulation forming; (5) arranging a pipeline at the bottom of the atomization box to be connected with a vertical cylindrical spiral separation device, connecting the lower end of the spiral separation device with a powder collecting tank, and connecting the side surface of the lower end with a pipeline of an exhaust fan; and (6) the particles in the powder collecting tank are screened, and the particles on the screen are collected to serve as the smelting flux. The method disclosed by the invention is safe in production operation; the formed welding flux particles are directly screened without mechanical crushing, and the welding flux particles are spherical and good in flowability; during submerged-arc welding, welding flux feeding is uniform, a molten pool is completely covered, the covering thickness is consistent, and the forming property, quality and mechanical property of a welding bead are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of flux smelting materials, and in particular to a preparation method of spherical smelting flux. Background Art

[0002] Melting flux is an indispensable material for submerged arc welding and electroslag welding, which affects the formability, quality and mechanical properties of the weld. At present, the manufacturing process of melting flux is to pour the flux melt directly into water and form it with water quenching. The water quenching forming process and products have the following shortcomings: the water quenching production operation is explosive and unsafe; the flux melt is easy to pulverize after rapid cooling by water quenching; the large particles after water quenching are irregular in shape and poor in fluidity after mechanical crushing. During submerged arc welding, it is easy to cause feed blockage, uneven feed, uneven thickness of flux coverage in the molten pool, and even leakage to produce open arc, causing weld porosity defects. In the iron and steel metallurgical industry, the steel slag air quenching method has achieved good application results. The melting flux is formed by air quenching. The flux melt can be cut into droplets, quickly cooled and solidified into spherical particles. The production operation is safe, the flux has good fluidity, and the welding production process is stable, which can provide a guarantee for obtaining high-quality and high-performance welds. Summary of the invention

[0003] In view of this, the present invention provides a method for preparing spherical molten flux. In view of the shortcomings of the existing molten flux water quenching method, the present invention provides a spherical molten flux air quenching granulation forming method. The method is safe in production and operation; the flux particles do not need to be mechanically crushed and directly screened after forming, and the flux particles are spherical and have good fluidity; during submerged arc welding, the flux is fed evenly, the molten pool covers the entire area with a consistent thickness, and the weld formability, quality and mechanical properties are guaranteed.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] A method for preparing a spherical melting flux comprises the following steps:

[0006] (1) Pretreatment of flux raw materials:

[0007] Stir and mix the designed flux ingredients evenly, and bake them in a heating furnace to remove moisture;

[0008] (2) Flux melting:

[0009] The dried flux raw materials are placed in a melting furnace preheated to a high temperature, heated and melted, and stirred to form a high-temperature flux melt;

[0010] (3) Intermediate packet flow control processing:

[0011] The flux melt flows into the tundish through the outlet trough of the smelting furnace, a dam is arranged in the tundish, and the flux melt flows into the outlet pipe at the bottom of the tundish through the overflow port prefabricated in the dam, and forms a flux melt jet at the outlet pipe port;

[0012] (4) Continuous air quenching granulation forming:

[0013] At the jet outlet, the flux melt jet is impacted by the high-pressure and high-speed air jet and cut into atomized droplets, which are rapidly cooled and solidified in the atomization box.

[0014] (5) Separation of flux particles and atomized gas:

[0015] A pipeline is arranged at the bottom of the atomizing box to be connected to the vertical cylindrical spiral separation device, the lower end of the spiral separation device is connected to the powder collecting tank, and the side of the lower end is connected to the pipeline of the exhaust fan;

[0016] (6) Flux particle screening and collection:

[0017] The particles in the powder collecting tank are screened and the particles on the screen are collected as smelting flux.

[0018] Preferably, in step (2), the flux is smelted in an electric arc furnace, a crucible resistance furnace or a flame furnace.

[0019] Preferably, in step (3), the temperature of the tundish is preheated to above 1000°C.

[0020] Preferably, in the step (3), a tundish with an overflow port on the intercepting dam is used to control and stabilize the flow, the overflow port has a diameter of 50 mm, and the inner diameter of the outlet pipe is 40 mm.

[0021] Preferably, in step (4), compressed air is used to impact the flux melt jet through a supersonic nozzle, and the compressed air pressure at the inlet end of the supersonic nozzle is greater than 0.7 MPa, and the flow rate is 0.7 to 1.5 m 3 / s, the gas velocity impacting the melt jet is Ma0.8~1.2, the inner diameter of the nozzle is 40mm, and the angle between the nozzle and the melt jet is between 30° and 90°.

[0022] Preferably, in step (5), a vertical cylindrical spiral separator is used to separate the atomized gas and the flux particles, and the particle size of the particles in the powder collecting tank is 0.06 to 3.2 mm.

[0023] Preferably, in step (6), sieving is performed using a 100-mesh sieve, and particles on the sieve are collected and used for melting flux.

[0024] Compared with the prior art, the present invention has achieved the following technical effects:

[0025] (1) The air quenching granulation production operation safety of the present invention is improved, and there is no explosion hazard;

[0026] (2) The air-quenched granulated particles of the present invention are not easy to pulverize, and can be directly screened and collected without mechanical crushing, with a high yield;

[0027] (3) The wind-quenched granules of the present invention are spherical and have good fluidity. During submerged arc welding, the flux is fed evenly without clogging. The molten pool is fully covered with a uniform thickness, and no open arc or weld porosity is generated. The metallurgical action between the flux and the molten pool is stable, and the weld composition is uniform and consistent. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of a method for preparing a spherical molten flux. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention adopts two representative spherical melting flux wind quenching granulation forming process methods. One is the model of submerged arc welding melting flux in the national standard, and the other is a self-developed melting flux.

[0031] Embodiment 1:

[0032] A method for preparing a spherical melting flux, characterized in that it comprises the following steps:

[0033] (1) Pretreatment of flux raw materials:

[0034] Stir and mix the designed flux ingredients evenly, and bake them in a heating furnace to remove moisture;

[0035] (2) Flux melting:

[0036] The dried flux raw materials are placed in a melting furnace preheated to a high temperature, heated and melted, and stirred to form a high-temperature flux melt;

[0037] Among them, flux melting adopts arc furnace, crucible resistance furnace and flame furnace;

[0038] (3) Intermediate packet flow control processing:

[0039] The flux melt flows into the tundish through the outlet trough of the smelting furnace, and a dam is set in the tundish with a preheating temperature of more than 1000°C. The flux melt flows into the outlet pipe at the bottom of the tundish through the overflow port prefabricated in the dam, and forms a flux melt jet at the outlet pipe port;

[0040] Among them, a tundish with an overflow port on the intercepting dam is used for flow control and stabilization. The overflow port has a diameter of 50 mm and the inner diameter of the outlet pipe is 40 mm.

[0041] (4) Continuous air quenching granulation forming:

[0042] At the jet outlet, the flux melt jet is impacted by the high-pressure and high-speed air jet and cut into atomized droplets, which are rapidly cooled and solidified in the atomization box.

[0043] Among them, compressed air is used to impact the flux melt jet through a supersonic nozzle. The compressed air pressure at the inlet end of the supersonic nozzle is greater than 0.7MPa, and the flow rate is 0.7~1.5m 3 / s, the gas velocity impacting the melt jet is Ma0.8~1.2, the inner diameter of the nozzle is 40mm, and the angle with the melt jet is between 30°~90°;

[0044] (5) Separation of flux particles and atomized gas:

[0045] A pipeline is arranged at the bottom of the atomizing box to be connected to the vertical cylindrical spiral separation device, the lower end of the spiral separation device is connected to the powder collecting tank, and the side of the lower end is connected to the pipeline of the exhaust fan;

[0046] Among them, a vertical cylindrical spiral separator is used to separate atomized gas and flux particles, and the particle size in the powder collecting tank is 0.06 to 3.2 mm;

[0047] (6) Flux particle screening and collection:

[0048] The particles in the powder collecting tank are screened, and the particles on the screen are collected as smelting flux;

[0049] Among them, sieve with a 100-mesh sieve, collect the particles on the sieve and use them as melting flux.

[0050] Embodiment 2:

[0051] According to the relevant provisions of F4A2-H08A in GB / T 5293-1999, spherical HJ431 melting flux is prepared by wind quenching method. According to the mass percentage of components MnO-26%, SiO2-45%, CaF2 -8%, MgO-5%, CaO-4%, TiO2-3%, Al2O3-3%, manganese ore, fluorite, magnesia, quicklime, quartz sand, rutile and appropriate amount of coke powder are taken, the mixed materials are dried and put into the furnace for melting. After the melt is melted, it is kept warm for 1 hour and injected into the tundish. Under the compressed air pressure of 0.7MPa and flow rate of 0.8m 3 / s conditions, the medium manganese high silicon low fluorine smelting flux of the present invention can be obtained by wind quenching and 100 mesh screening.

[0052] Embodiment 3:

[0053] In this embodiment, the spherical smelting flux is prepared by the wind quenching method of laterite nickel slag. The statistical results of multiple batches of composition detection of laterite nickel ore thermal furnace slag from a long-process stainless steel smelting company in Beihai City, Guangxi Zhuang Autonomous Region are shown in Table 1: Table 1: Statistical results of multiple batches of composition detection of laterite nickel ore thermal furnace slag from a long-process stainless steel smelting company in Beihai City, Guangxi Zhuang Autonomous Region

[0054]

[0055] Take 40% of the above-mentioned laterite nickel ore slag, 40% of manganese ore, 8% of fluorite, 8% of quartz sand and 4% of rutile according to mass percentage, mix them evenly and dry them, put them into the furnace for smelting, keep the melt warm for 1h after it is cleared, and inject it into the tundish. 3 / s conditions, the spherical medium-manganese, medium-silicon and low-fluorine smelting flux of the present invention can be obtained by wind quenching and 100-mesh screening.

[0056] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a spherical melting flux, characterized in that: The following steps are involved: (1) Pretreatment of flux raw materials: Stir and mix the designed flux ingredients evenly, and bake them in a heating furnace to remove moisture; (2) Flux melting: The dried flux raw materials are placed in a melting furnace preheated to a high temperature, heated and melted, and stirred to form a high-temperature flux melt; (3) Intermediate packet flow control processing: The flux melt flows into the tundish through the outlet trough of the smelting furnace, a dam is arranged in the tundish, and the flux melt flows into the outlet pipe at the bottom of the tundish through the overflow port prefabricated in the dam, and forms a flux melt jet at the outlet pipe port; (4) Continuous air quenching granulation forming: At the jet outlet, the flux melt jet is impacted by the high-pressure and high-speed air jet and cut into atomized droplets, which are rapidly cooled and solidified in the atomization box. (5) Separation of flux particles and atomized gas: A pipeline is arranged at the bottom of the atomizing box to be connected to the vertical cylindrical spiral separation device, the lower end of the spiral separation device is connected to the powder collecting tank, and the side of the lower end is connected to the pipeline of the exhaust fan; (6) Flux particle screening and collection: The particles in the powder collecting tank are screened and the particles on the screen are collected as smelting flux.

2. The method for preparing a spherical melting flux according to claim 1, characterized in that: In the step (2), the flux is smelted in an electric arc furnace, a crucible resistance furnace or a flame furnace.

3. The method for preparing a spherical melting flux according to claim 1, characterized in that: In the step (3), the temperature of the tundish is preheated to above 1000°C.

4. The method for preparing a spherical melting flux according to claim 1, characterized in that: In the step (3), a tundish with an overflow port on the intercepting dam is used to control and stabilize the flow, the overflow port has a diameter of 50 mm, and the inner diameter of the outlet pipe is 40 mm.

5. The method for preparing a spherical melting flux according to claim 1, characterized in that: In the step (4), compressed air is used to impact the flux melt jet through a supersonic nozzle, and the compressed air pressure at the inlet end of the supersonic nozzle is greater than 0.7 MPa, and the flow rate is 0.7 to 1.5 m 3 / s, the gas velocity impacting the melt jet is Ma0.8~1.2, the inner diameter of the nozzle is 40mm, and the angle between the nozzle and the melt jet is between 30° and 90°.

6. The method for preparing a spherical melting flux according to claim 1, characterized in that: In the step (5), a vertical cylindrical spiral separator is used to separate the atomized gas and the flux particles, and the particle size of the particles in the powder collecting tank is 0.06 to 3.2 mm.

7. The method for preparing a spherical melting flux according to claim 1, characterized in that: In the step (6), the mixture is sieved with a 100-mesh sieve, and the particles on the sieve are collected and used for melting flux.