Method for preparing granularity-controllable iron phosphate by utilizing iron phosphate dust collection material recovered from mother liquor

Through mother liquor recycling and regulating the molar ratio of elements, combined with the heating synthesis method of seed crystal additives, the problems of high costs and waste of resources in ferric phosphate synthesis are solved, low-cost, efficient production and controllable particle size of iron phosphate are achieved, and lithium is improved Battery performance.

CN118929600AActive Publication Date: 2024-11-12YICHANG BRUNP RECYCLING TECH CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411167009.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

In the existing iron phosphate synthesis methods, the cost is high, the resource waste is severe during the production process, the wastewater treatment cost is high, and the particle size is unstable, which affects the performance of lithium batteries.

Method used

The iron phosphate dust collecting material is recovered through the mother liquor, the Fe/P and S/Fe molar ratio is controlled, the seed additive is added, and the temperature is synthesised, so as to achieve stable particle size control of anhydrous iron phosphate, reduce the consumption of auxiliary materials, and improve resource utilization.

Benefits of technology

It realizes low-cost and efficient production of iron phosphate, controllable particle size, reduces waste and wastewater treatment costs, improves the recovery rate of iron phosphate and lithium battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929600A_ABST
    Figure CN118929600A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing granularity-controllable iron phosphate by recovering an iron phosphate dust collection material from a mother liquor, which comprises the following steps: S1, washing and drying the iron phosphate dust collection material, then carrying out primary roasting, mixing the obtained roasted material with the iron phosphate synthesis mother liquor, pulping, and carrying out solid-liquid separation to obtain an anti-dissolving metal solution; s2, the anti-dissolution metal solution and the phosphorus iron slag acid-dissolution metal solution are mixed, the molar ratio of Fe to P in the obtained mixed solution is adjusted to be (0.75-0.95): 1, the molar ratio of S to Fe in the obtained mixed solution is adjusted to be (1-1.3): 1, and a mixed phosphorus iron solution is obtained; s3, the mixed ferrophosphorus solution is heated, a seed crystal additive is added in the heating process, heat preservation is carried out after heating is completed, iron phosphate slurry is obtained, solid-liquid separation is carried out on the iron phosphate slurry, an obtained solid phase is subjected to secondary roasting, and anhydrous iron phosphate is obtained. According to the method, the granularity of the anhydrous iron phosphate is stable and controllable through a regulation and control means, the waste materials generated in the iron phosphate production process are recycled, and recycling of the waste materials is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferric phosphate synthesis, and particularly relates to a method for preparing ferric phosphate with controllable particle size by recycling ferric phosphate dust collecting material with mother liquor. Background Art

[0002] Currently in the new energy power lithium battery industry, the development of low-cost, long-life and safe and fast-charging batteries has become two key technologies. Lithium iron phosphate batteries have shown great application potential and market prospects in the fields of energy storage and power applications due to their advantages in safety, environmental protection and applicability of primary technology. However, their cost is relatively high, and the battery cost mainly comes from the high cost of positive electrode materials. In order to reduce the cost of battery materials, the process is mainly optimized and improved from the perspective of the synthesis of positive electrode material precursor iron phosphate.

[0003] The current existing methods for synthesizing iron phosphate include the sodium method: ferrous sulfate plus sodium hydroxide, phosphoric acid and hydrogen peroxide. This method will produce sodium sulfate in a high concentration during the production process. This byproduct is not valuable, and the processing cost will restrict the production of iron phosphate. Therefore, how to prepare low-cost and high-performance iron phosphate is crucial for lithium iron phosphate. And as a precursor of lithium iron phosphate batteries, the performance indicators of iron phosphate have a great influence on the performance of lithium iron phosphate batteries, and the particle size of iron phosphate also has a certain influence on the grinding efficiency of lithium iron phosphate.

[0004] In the recovery and treatment of the mother liquor of ammonium / sodium method synthetic iron phosphate, calcium hydrogen phosphate is added to mix and make pulp, sulfuric acid is added to the pulp, and then it is filtered and calcium hydrogen phosphate is added multiple times, and ammonia water or sodium hydroxide is added to adjust the pH value, filter and other processes to obtain calcium sulfate gypsum; however, this method requires the additional introduction of elemental calcium, and new process treatment is required for wastewater treatment, resulting in increased treatment costs; and in the entire production system, the P element cannot be fully recycled and utilized, and the cost of wastewater treatment is also high.

[0005] In the normal production process of iron phosphate, the main components of the dust collection material in the bag of the rotary kiln are anhydrous iron phosphate carrying a large amount of flue gas and some dihydrate iron phosphate that has not been successfully crystallized. The dihydrate and anhydrous iron phosphate cannot be used because of their high S content, unqualified BET, small particle size, or agglomeration. The main current treatment methods for rotary kiln bag dust collection materials are: (1) the rotary kiln bag dust collection materials are collected through the silo and returned to the front end for acid dissolution reaction with sulfuric acid to dissolve the anhydrous iron phosphate therein to obtain an iron phosphate solution, and then precipitated dihydrate iron phosphate is obtained by a synthetic method. This method can obtain a product with a relatively stable specific surface area and particle size. However, due to the large amount of flue gas attachments carried on the surface of the bag dust collection materials, the S content in the molten metal is relatively high. The S content in the synthesized dihydrate iron phosphate is relatively high and cannot be completely removed during the roasting process. In this method, the rotary kiln bag dust collection materials are mainly composed of anhydrous iron phosphate carrying a large amount of flue gas and dihydrate iron phosphate that has not been successfully crystallized. During the entire sulfuric acid dissolution process, the dihydrate iron phosphate cannot be completely dissolved, and a large amount of remaining dihydrate iron phosphate material cannot be removed. Recovery, and it is impossible to achieve complete separation, which will reduce the filter pressing efficiency during the dissolution and filtration process, affecting the production rhythm; (2) the rotary kiln bag dust collection material is screened and then water is added to make pulp to obtain anhydrous iron phosphate filter cake, the anhydrous iron phosphate filter cake and phosphoric acid solution are mixed, heated, recrystallized, and dihydrate iron phosphate is obtained, and then solid-liquid separation is performed to obtain dihydrate iron phosphate filter cake, and then dried and roasted to finally obtain anhydrous iron phosphate. However, this method requires the addition of a large amount of high-concentration phosphoric acid to dissolve the dihydrate iron phosphate during the dissolution of the bag dust collection material, resulting in a large amount of auxiliary material consumption. In addition, after the dissolution is completed in this process, the acidity of the mother liquor generated is greatly reduced and cannot be recovered. A large amount of phosphoric acid exists in the mother liquor, resulting in a serious waste of phosphorus resources, and it is impossible to achieve complete recovery of waste materials and wastewater. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a method for preparing iron phosphate with controllable particle size by recycling iron phosphate dust collection material with mother liquor, in which the mother liquor is fully circulated to dissolve and roast the dust collection material during the entire production process, and the particle size of anhydrous iron phosphate is stably controlled by means of regulation.

[0007] According to a first aspect of the present invention, a method for preparing ferric phosphate with controllable particle size by recycling ferric phosphate dust collecting material using mother liquor is proposed, comprising the following steps:

[0008] S1: washing and drying the iron phosphate dust collection material and then calcining it once, mixing the calcined material with the iron phosphate synthesis mother liquor to prepare a slurry, and obtaining an anti-dissolved metal solution after solid-liquid separation;

[0009] S2: mixing the reverse-dissolved metal solution with the ferrophosphorus slag acid-dissolved metal solution, adjusting the Fe / P molar ratio in the obtained mixed solution to (0.75-0.95):1, and the S / Fe molar ratio to (1-1.3):1, to obtain a mixed ferrophosphorus solution;

[0010] S3: heating the mixed ferrophosphorus solution, adding a seed additive during the heating process, maintaining the temperature after the heating is completed to obtain ferrophosphate slurry, performing solid-liquid separation on the ferrophosphate slurry, and performing secondary roasting on the obtained solid phase to obtain anhydrous ferric phosphate.

[0011] It should be noted that the "Fe / P molar ratio" and "S / Fe molar ratio" in the present invention refer to the molar ratio of the corresponding elements, rather than the molar ratio between single substances.

[0012] In some embodiments, in step S1, the iron phosphate dust collecting material includes anhydrous iron phosphate and dihydrate iron phosphate, and the sulfur content of the iron phosphate dust collecting material is 10000-20000 ppm.

[0013] In some preferred embodiments, the iron phosphate dust collection material is the rotary kiln bag dust collection material in the iron phosphate sintering process. The dust collection material is collected by back-blowing the bag dust collector, and has two main components, one is anhydrous iron phosphate, accounting for about 70%; the other is dihydrate iron phosphate that is not completely crystallized during the roasting process, accounting for about 30%.

[0014] In some embodiments, in step S1, the washing process includes: adding water to the iron phosphate dust collecting material to prepare a slurry, controlling the solid content of the slurry to be 25% to 35%, and then performing filter pressing and washing to obtain a dust collecting material filter cake. The washing can remove impurities with a high S content attached to the surface of the iron phosphate dust collecting material.

[0015] In some embodiments, in step S1, the temperature of the primary calcination is 500-600°C and the time is 1-2 hours. The dried dust collection filter cake is calcined to obtain anhydrous iron phosphate with uniform particle size and complete crystal transformation. The anhydrous phosphoric acid has an abnormal BET and cannot be directly used. It can be dissolved and reused by using a highly acidic iron phosphate synthesis mother liquor.

[0016] In some embodiments, in step S1, the pH of the iron phosphate synthesis mother liquor is less than 1; and / or, during the mixed pulping process, the solid content of the pulp is controlled to be 10% to 25%.

[0017] In some embodiments, in step S1, the S content of the ferric phosphate synthesis mother liquor is greater than 40 g / L.

[0018] In some preferred embodiments, step S1 further comprises heating and stirring the mixed slurry, wherein the heating is to raise the temperature to 40-60° C., the stirring speed is 200-400 r / min, and the stirring time is 8-10 h.

[0019] In some embodiments, in step S2, the reverse molten metal solution is mixed with the ferrophosphorus slag acid-soluble metal solution at a volume ratio of 1:4 to 1:2; the Fe / P molar ratio of the ferrophosphorus slag acid-soluble metal solution is (0.75-0.95):1, and the S / Fe molar ratio is (1-1.3):1. The ferrophosphorus slag acid-soluble metal solution can be a metal solution obtained by acid-dissolving and removing impurities from lithium iron phosphate slag.

[0020] In some embodiments, the Fe content in the ferrophosphorus slag acid-soluble metal liquid is 65-75 g / L, and the P content is 45-55 g / L.

[0021] In some embodiments, in step S2, the Fe / P molar ratio in the obtained mixed solution is adjusted to (0.75-0.95):1, and the S / Fe molar ratio is adjusted to (1-1.3):1, including: using phosphoric acid with a mass fraction of 70%-85% to adjust the Fe / P molar ratio in the system to (0.75-0.95):1, and using concentrated sulfuric acid with a mass fraction of about 98% to adjust the S / Fe molar ratio in the system to (1-1.3):1. In the mixed ferrophosphorus solution, phosphate radicals may be slightly excessive to increase the precipitation rate of iron, and in subsequent processes, the excess phosphoric acid in the mother liquor may be recycled by recovering the mother liquor, and the Fe / P molar ratio may be specifically any one of 0.75, 0.8, 0.85, 0.9, and 0.95 or any value between any two of them; the particle size of the ferric phosphate may be controlled by adjusting the S / Fe molar ratio, and the particle size of the ferric phosphate generated by the subsequent reaction step gradually decreases with the increase of the S / Fe molar ratio, and the S / Fe molar ratio may be specifically any one of 1.02, 1.08, 1.13, 1.18, and 1.23 or any value between any two of them.

[0022] In some embodiments, in step S2, the concentration of Fe in the mixed ferrophosphorus solution is 60-75 g / L. The concentration of Fe in the mixed ferrophosphorus solution can be any one of 65 g / L, 70 g / L, 72 g / L, 75 g / L, or any value between any two of them.

[0023] In some embodiments, in step S3, the heating process includes: heating to 85-95°C at a rate of 10°C / h to 30°C / h, and then keeping warm for 10-20h. The heating rate can be any one of 10°C / h, 15°C / h, 20°C / h, 30°C / h, or any value between any two; the temperature of ferric phosphate synthesis is 85-95°C, specifically any one of 85°C, 90°C, 95°C, or any value between any two; the holding time can be any one of 10h, 15h, 20h, or any value between any two. Controlling the heating rate within this range can control the particle size D50 of the product ferric phosphate between 3.5 and 6.5μm, otherwise it may cause particle size deviation.

[0024] In some embodiments, in step S3, the seed additive is added when the mixed ferrophosphorus solution is heated to 50-60°C.

[0025] In some embodiments, in step S3, the seed additive is an iron phosphate slurry with a solid content of 20% to 40%; and / or the particle size D50 of the seed additive is 1 to 1.5 μm. The solid content of the seed additive can be any one of 25%, 30%, 35%, 40%, or any value between any two of them.

[0026] In some embodiments, in step S3, the mass of the seed additive is 5% to 20% of the mass of the mixed ferrophosphorus solution.

[0027] In some embodiments, in step S3, the solid-liquid separation includes a primary filter press washing and a secondary filter press washing.

[0028] In some embodiments, the solid phase washed by the first filter press is used to prepare the seed crystal additive. The seed crystal additive is prepared from ferric phosphate dihydrate generated during the temperature rise synthesis process, and the internal circulation of the seed crystal can be realized.

[0029] In some embodiments, in step S3, the seed additive is obtained by: performing a filter press and washing on the iron phosphate slurry to obtain an iron phosphate filter cake, adding water to make pulp to obtain a secondary slurry, and sand milling the secondary slurry; wherein the solid content of the secondary slurry is 20% to 40%, and the speed of the sand mill is 300 to 500 r / min. By using the seed additive obtained by sand milling the dihydrate iron phosphate slurry synthesized in the later stage to induce the synthesis of the iron phosphate, the introduction of impurities can be avoided and the cost of auxiliary materials can be reduced.

[0030] In some embodiments, in step S3, after the ferric phosphate slurry is subjected to solid-liquid separation, the obtained mother liquor is used to slurry the roasted material in step S1.

[0031] In some embodiments, in step S3, the solid-liquid separation process includes: using washing water to filter-wash the iron phosphate slurry multiple times, each time the volume ratio of the iron phosphate slurry to the washing water is (1:1) to (1:3), until the pH of the washing water after washing is ≥3.

[0032] In some embodiments, in step S3, before the secondary calcination, the solid phase obtained by solid-liquid separation is dried at a temperature of 120 to 150° C. The specific drying temperature may be any one of 120° C., 130° C., 140° C., 150° C., or any value between any two of them.

[0033] In some embodiments, in step S3, the secondary calcination temperature is 650-750°C and the time is 40-60 min. The secondary calcination temperature can be any one of 650°C, 700°C, 750°C or any value in between.

[0034] In some embodiments, step S3 further comprises screening and demagnetizing the anhydrous ferric phosphate and packaging the resulting product.

[0035] According to a second aspect of the present invention, there is provided an iron phosphate which is prepared by the method described in the first aspect of the present invention, wherein the particle size D50 of the iron phosphate is 3.5 to 6.5 μm.

[0036] According to the third aspect of the present invention, the application of the method described in the first aspect of the present invention in the production of iron phosphate is proposed. The present invention recycles the roasted dust collected during the synthesis of iron phosphate, and completely recycles the mother liquor to prepare iron phosphate with controllable particle size. The method of the present invention recycles the waste generated during the production of iron phosphate, realizes the resource utilization of the waste, and reduces the treatment cost of solid waste.

[0037] According to one embodiment of the present invention, there are at least the following beneficial effects:

[0038] 1. The present invention adjusts the element ratio in the mixed ferrophosphorus solution and adds a seed additive during the heating synthesis process of ferrophosphate, so that the particle size of the ferrophosphate product is stable and controllable.

[0039] 2. The present invention belongs to a green and environmentally friendly synthesis method for ferric phosphate induced by seed crystals without the introduction of other cations. The present invention introduces ferrophosphorus slag acid-soluble metal liquid as raw material, and mixes it with the reverse soluble metal solution obtained by dissolving ferric phosphate dust collection material roasting material in ferric phosphate synthesis mother liquor, and uses seed crystal additives to induce crystallization to synthesize ferric phosphate, thereby reducing the process flow and avoiding the problems of introducing other metal cations into the mother liquor, which leads to the enrichment of impurities in the mother liquor, the inability to reuse the mother liquor, the increase of wastewater treatment cost and the certain impact of external discharge treatment on the environment.

[0040] 3. Compared with the traditional process, this process adds mother liquor and waste disposal and recycling processes. The anti-dissolved metal solution after the mother liquor dissolves the dust collector in the rotary kiln bag is mixed with the acid-dissolved metal solution of ferrophosphorus slag and adjusted, and iron phosphate synthesis is carried out again. In the synthesis process, the excess sulfuric acid and phosphoric acid in the mother liquor and the Fe in the waste are recycled multiple times. The reuse of the dust collector in the bag improves the recovery rate of P and Fe in the production process, realizes full utilization of resources, and greatly reduces the unit production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0042] Figure 1 This is a SEM image of the anhydrous ferric phosphate prepared in Example 1 of the present invention magnified 50,000 times;

[0043] Figure 2 This is a SEM image of the anhydrous ferric phosphate prepared in Example 1 of the present invention magnified 10,000 times;

[0044] Figure 3 This is a SEM image of the anhydrous ferric phosphate prepared in Example 1 of the present invention magnified 5000 times;

[0045] Figure 4 This is a SEM image of the anhydrous ferric phosphate prepared in Example 1 of the present invention magnified 2500 times;

[0046] Figure 5 This is a production process flow chart of Example 1 of the present invention;

[0047] Figure 6 This is the XRD diagram of the anhydrous ferric phosphate prepared in Examples 1-5 of the present invention. DETAILED DESCRIPTION

[0048] The concept and technical effects of the present invention will be clearly and completely described below in conjunction with embodiments to fully understand the purpose, features and effects of the present invention.

[0049] Unless otherwise specified, the raw materials, reagents or devices used in the following embodiments can be obtained from conventional commercial channels or by existing known methods. Among them, the bag dust collection material includes anhydrous iron phosphate (about 67% by mass), dihydrate iron phosphate that has not been completely crystallized during the roasting process (about 30% by mass), and also includes 3% sulfur; the ferrophosphorus slag acid-dissolved metal liquid is the metal liquid after the lithium iron phosphate slag is acid-dissolved and impurities are removed, and the main impurities are Al and Cu, with an Al content of 0.2g / L and a Cu content of 10mg / L.

[0050] Example 1

[0051] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling mother liquor from dust collecting materials in rotary kiln bags, such as Figure 5 As shown, the specific steps include:

[0052] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0053] (2) A 40% volume fraction of the bottom liquid mother liquor (Fe content is 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining volume fraction of the bottom liquid mother liquor of 60% is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After filtration, the reversed gold is obtained. The ferrophosphorus slag acid-soluble metal liquid N1 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.023) is mixed and stirred with the anti-soluble metal solution M1 for 4 hours, and the two metal liquids M1:N1 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.023 to obtain a mixed ferrophosphorus solution Q1.

[0054] (3) Add the mixed ferrophosphorus solution Q1 mixed at the front end to the reactor and start heating, control the heating rate to 10°C / h, and the stirring rate of the reactor to 350r / min. When the temperature reaches 50°C, start adding the seed additive, the mass of which is 10% of the mass of the mixed ferrophosphorus solution Q1, the solid content of which is 28%, and the particle size D50 is 1.0μm. Control the addition time of the seed additive to be within 30min, and start the reactor insulation after the temperature reaches 95°C, and the insulation time is 20h.

[0055] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A1 is obtained by screening, demagnetization and packaging.

[0056] The SEM image of anhydrous ferric phosphate prepared in this embodiment is as follows: Figure 1-4 As shown, it can be seen that the synthesized anhydrous ferric phosphate is relatively stable in particle size and morphology.

[0057] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0058] Example 2

[0059] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling dust collected by rotary kiln bags using mother liquor, which specifically includes the following steps:

[0060] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0061] (2) A 40% volume fraction of the bottom liquid mother liquor (Fe content is 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining volume fraction of the bottom liquid mother liquor of 60% is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After filtration, the reversed gold is obtained. The ferrophosphorus slag acid-soluble metal liquid N2 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.089) is mixed and stirred with the anti-soluble metal solution M2 for 4 hours. The two metal liquids M2:N2 are mixed in a volume ratio of 1:2. The final Fe concentration is 72g / L and the P concentration is 49.8g / L. Then, 85% mass fraction phosphoric acid is used to adjust n(Fe):n(P)=0.8; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.089 to obtain a mixed ferrophosphorus solution Q2.

[0062] (3) Add the mixed ferrophosphorus solution Q2 mixed at the front end to the reactor and start heating, control the heating rate to 10°C / h, and the stirring rate of the reactor to 350r / min. When the temperature reaches 50°C, start adding the seed additive, the mass of which is 10% of the mass of the mixed ferrophosphorus solution Q2, the solid content of which is 28%, and the particle size D50 is 1.0μm. Control the addition time of the seed additive to be within 30min, and start the reactor insulation after the temperature reaches 95°C, and the insulation time is 20h.

[0063] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A2 is obtained by screening, demagnetization and packaging.

[0064] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0065] Example 3

[0066] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling dust collected by rotary kiln bags using mother liquor, which specifically includes the following steps:

[0067] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0068] (2) A 40% by volume bottom liquid mother liquor (Fe content is 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining 60% by volume bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M3; the ferrophosphorus slag acid-dissolved metal solution N3 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.13) and the anti-dissolved metal solution M3 are mixed and stirred for 4 hours, and the two metal liquids M3:N3 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L, and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.13 to obtain a mixed ferrophosphorus solution Q3.

[0069] (3) Add the mixed ferrophosphorus solution Q3 mixed at the front end to the reactor and start heating. The heating rate is controlled to be 10°C / h, and the stirring rate of the reactor is 350r / min. When the temperature reaches 50°C, the seed additive is added. The mass of the seed additive is 10% of the mass of the mixed ferrophosphorus solution Q3, the solid content of the seed additive is 28%, and the particle size D50 is 1.0μm. The seed additive addition time is controlled within 30min. After the temperature is raised to 95°C, the reactor is kept warm for 20h.

[0070] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A3 is obtained by screening, demagnetization and packaging.

[0071] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0072] Example 4

[0073] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling dust collected by rotary kiln bags using mother liquor, which specifically includes the following steps:

[0074] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0075] (2) A 40% by volume bottom liquid mother liquor (Fe content is 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining volume of 60% bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M4; the ferrophosphorus slag acid-dissolved metal solution N4 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.18) and the anti-dissolved metal solution M4 are mixed and stirred for 4 hours, and the two metal liquids M4:N4 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L, and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.18 to obtain a mixed ferrophosphorus solution Q4.

[0076] (3) Add the mixed ferrophosphorus solution Q4 mixed at the front end to the reactor and start heating. The heating rate is controlled to be 10°C / h, and the stirring rate of the reactor is 350r / min. When the temperature reaches 50°C, the seed additive is added. The mass of the seed additive is 10% of the mass of the mixed ferrophosphorus solution Q4, the solid content of the seed additive is 28%, and the particle size D50 is 1.0μm. The seed additive addition time is controlled within 30min. After the temperature reaches 95°C, the reactor is kept warm for 20h.

[0077] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A4 is obtained by screening, demagnetization and packaging.

[0078] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0079] Example 5

[0080] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling dust collected by rotary kiln bags using mother liquor, which specifically includes the following steps:

[0081] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0082] (2) A 40% by volume bottom liquid mother liquor (Fe content is 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining 60% by volume bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M5; the ferrophosphorus slag acid-dissolved metal solution N5 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.23) and the anti-dissolved metal solution M5 are mixed and stirred for 4 hours, and the two metal liquids M5:N5 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L, and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.23 to obtain a mixed ferrophosphorus solution Q5.

[0083] (3) Add the mixed ferrophosphorus solution Q5 mixed at the front end to the reactor and start heating, control the heating rate to 10°C / h, and the stirring rate of the reactor to 350r / min. When the temperature reaches 50°C, start adding the seed additive, the mass of which is 10% of the mass of the mixed ferrophosphorus solution Q5, the solid content of which is 28%, and the particle size D50 is 1.0μm. Control the time of adding the seed additive to be within 30min, and start the reactor insulation after the temperature reaches 95°C, and the insulation time is 20h.

[0084] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A5 is obtained by screening, demagnetization and packaging.

[0085] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0086] Example 6

[0087] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling dust collected by rotary kiln bags using mother liquor, which specifically includes the following steps:

[0088] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0089] (2) A 40% by volume bottom liquid mother liquor (Fe content is about 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining 60% by volume of the bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M6; the ferrophosphorus slag acid-dissolved metal solution N6 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.18) and the anti-dissolved metal solution M6 are mixed and stirred for 4 hours, and the two metal liquids M6:N6 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L, and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.18 to obtain a mixed ferrophosphorus solution Q6.

[0090] (3) Add the mixed ferrophosphorus solution Q6 mixed at the front end to the reactor and start heating. The heating rate is controlled to be 30°C / h, and the stirring rate of the reactor is 350r / min. When the temperature reaches 50°C, the seed additive is added. The mass of the seed additive is 10% of the mass of the mixed ferrophosphorus solution Q6, the solid content of the seed additive is 28%, and the particle size D50 is 1.0μm. The seed additive addition time is controlled within 30min. After the temperature is raised to 95°C, the reactor is kept warm for 20h.

[0091] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A6 is obtained by screening, demagnetization and packaging.

[0092] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0093] Comparative Example 1

[0094] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling dust collected by rotary kiln bag by using mother liquor, which is different from that of embodiment 4 in that the heating rate in step (3) is 50° C. / h, and specifically comprises the following steps:

[0095] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0096] (2) A 40% by volume bottom liquid mother liquor (Fe content is about 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining 60% by volume of the bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M7; the ferrophosphorus slag acid-dissolved metal solution N7 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.18) and the anti-dissolved metal solution M7 are mixed and stirred for 4 hours, and the two metal liquids M7:N7 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L, and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.18 to obtain a mixed ferrophosphorus solution Q7.

[0097] (3) Add the mixed ferrophosphorus solution Q7 mixed at the front end to the reactor and start heating. The heating rate is controlled to be 50°C / h, and the stirring rate of the reactor is 350r / min. When the temperature reaches 50°C, the seed additive is added. The mass of the seed additive is 10% of the mass of the mixed ferrophosphorus solution Q7, the solid content of the seed additive is 28%, and the particle size D50 is 1.0μm. The seed additive addition time is controlled within 30min. After the temperature is raised to 95°C, the reactor is kept warm for 20h.

[0098] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A7 is obtained by screening, demagnetization and packaging.

[0099] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0100] Comparative Example 2

[0101] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling mother liquor from dust collecting materials in rotary kiln bags. The difference from Embodiment 4 is that the heating rate in step (3) is 50° C. / h, and the seed additive is added at 25° C., which specifically comprises the following steps:

[0102] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0103] (2) A 40% by volume bottom liquid mother liquor (Fe content is about 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining 60% by volume of the bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M8; the ferrophosphorus slag acid-dissolved metal solution N8 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.18) and the anti-dissolved metal solution M8 are mixed and stirred for 4 hours, and the two metal liquids M8:N8 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.18 to obtain a mixed ferrophosphorus solution Q8.

[0104] (3) Add the mixed ferrophosphorus solution Q8 mixed at the front end to the reactor, start adding the seed additive at room temperature (25°C), and start heating at the same time, control the heating rate to 50°C / h, and the stirring rate of the reactor to 350r / min. The mass of the seed additive is 10% of the mass of the mixed ferrophosphorus solution Q8, the solid content of the seed additive is 28%, and the particle size D50 is 1.0μm. Control the seed additive addition time within 30min, and start the reactor insulation after heating to 95°C, and the insulation time is 20h.

[0105] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A8 is obtained by screening, demagnetization and packaging.

[0106] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0107] Comparative Example 3

[0108] This embodiment provides a method for preparing ferric phosphate with controllable particle size by recycling mother liquor from dust collecting materials in rotary kiln bags. The difference from Embodiment 4 is that the heating rate in step (3) is 50° C. / h, and the seed additive is added at 90° C., which specifically comprises the following steps:

[0109] (1) The bag dust collection material was slurried with pure water to prepare a slurry with a solid content of 32%, and stirred in a tank for 4 hours; the slurry after slurrying was pumped into a filter press for filter pressing, washing, drying and calcining at 550°C for 2 hours to obtain a particle size D50 of 4.8 μm and a BET of 5.5 μm. 2 / g of anhydrous iron phosphate.

[0110] (2) A 40% by volume bottom liquid mother liquor (Fe content is about 3 g / L, S content is 50 g / L, P content is 12 g / L, Al content is 0.18 g / L, Cu content is 10 mg / L) with a pH value below 1 is injected into the dissolution tank, and the dust collection material that has been washed, dried, and roasted at the front end is added. After being completely dispersed, the remaining 60% by volume of the bottom liquid mother liquor is added for acid dissolution. The solid content of the slurry is controlled to be 25%, the acid dissolution temperature is 50°C, and the slurry is stirred at a rate of 400 r / min for 6 hours. After suction filtration, the reverse solution is obtained. Metal solution M9; the ferrophosphorus slag acid-dissolved metal solution N9 (molar ratio n(Fe):n(P)=0.8, n(S):n(Fe)=1.18) and the anti-dissolved metal solution M9 are mixed and stirred for 4 hours, and the two metal liquids M9:N9 are mixed in a volume ratio of 1:2, and the final Fe concentration is 72g / L and the P concentration is 49.8g / L, and then n(Fe):n(P)=0.8 is adjusted with 85% mass fraction of phosphoric acid; 98% concentrated sulfuric acid is used to adjust n(S):n(Fe)=1.18 to obtain a mixed ferrophosphorus solution Q9.

[0111] (3) Add the mixed ferrophosphorus solution Q9 mixed at the front end to the reactor and start heating. The heating rate is controlled to be 50°C / h. The stirring rate of the reactor is 350r / min. When the temperature reaches 90°C, the seed additive is added. The mass of the seed additive is 10% of the mass of the mixed ferrophosphorus solution Q9. The solid content of the seed additive is 28%, and the particle size D50(1) is 1.0μm. The seed additive addition time is controlled within 30min. After the temperature reaches 95°C, the reactor is kept warm for 20h.

[0112] (4) The obtained white powder slurry is run to a membrane filter press for a filter press washing, the volume ratio of slurry to washing water is 1:2, the mother liquor is collected separately and reused in step (2) for dissolving dust collecting material, and the filter cake can be used to prepare the seed additive in step (3) after unloading. The filter cake not used for preparing the seed additive is pulped and then subjected to a second filter press washing, the volume ratio of slurry to washing water is 1:3, and the pH of the washing water after washing is 3. The filter cake is conveyed to a paddle dryer by a belt for drying, the drying temperature is 130°C, the time is 1h, and the moisture content of the material after drying is controlled to be below 0.5%, and then the material is roasted, the rotary kiln roasting temperature is controlled at 700°C, and the material stays in the kiln for 60min to obtain anhydrous iron phosphate after complete roasting. Finally, the anhydrous iron phosphate A9 is obtained by screening, demagnetization and packaging.

[0113] The seed additive is an iron phosphate slurry with a solid content of 28% and a particle size D50 of 1.0 μm. The method for preparing the seed additive using the filter cake after a filter press washing comprises: taking the filter cake after a filter press washing, mixing it evenly by adding water to make a slurry, and then sand grinding it. During the slurry making process, the solid content of the slurry is controlled to be 28%, the sand milling speed is controlled to be 500 r / min, and the final particle size D50 is controlled to be 1.0 μm during the sand milling process to obtain the seed additive for use.

[0114] Test example

[0115] Data detection was performed on the iron phosphate prepared in Examples 1-6 and Comparative Examples 1-3. The test results are shown in Table 1:

[0116] Table 1 Iron phosphate detection data table

[0117]

[0118] It can be seen from Examples 1-5 that the particle size of iron phosphate changes significantly, and the particle size can be controlled by the S / Fe molar ratio. The particle size D50 gradually decreases with the increase of the S / Fe molar ratio. According to the detected data, the Fe and P contents and the Fe / P molar ratio of the obtained iron phosphate product are all within the theoretical range (Fe content is 36.1% to 36.7%, P content is 20.3% to 21%, and Fe / P molar ratio is between 0.97 and 0.99), and there is no significant difference; the BET and S content indicators are slightly different in Examples 1-5, but are still within the normal range (BET is between 4 and 7.5 m 2 / g, S content ≤500ppm).

[0119] It can be seen from Example 4, Example 6 and Comparative Example 1 that in the process of synthesizing iron phosphate, the particle size D50 of the product will increase as the heating rate is increased, but too fast a heating rate will result in too large a particle size D50, and the diffraction peak coincidence degree after subsequent sintering of lithium iron phosphate is low, which is not conducive to the performance of the electrochemical properties of the material. It can also be seen that too fast a heating rate will also increase the fluctuation of the product particle size, and in the subsequent sintering process of lithium iron phosphate, too large a particle size fluctuation will result in unstable sintering effect.

[0120] It can be seen from Comparative Examples 1, 2 and 3 that in the process of synthesizing ferric phosphate, the higher the temperature when the seed additive is added, the higher the particle size D50 of the product. If the temperature when the seed additive is added is too high, the fluctuation of the product particle size will also become larger.

[0121] Figure 6 This is the XRD diagram of the anhydrous ferric phosphate prepared in Example 1-5. It can be seen that the anhydrous ferric phosphate prepared in the present invention has good crystallinity.

[0122] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A method for preparing ferric phosphate with controllable particle size by recycling ferric phosphate dust collecting material using mother liquor, It is characterized in that The following steps are involved: S1: washing and drying the iron phosphate dust collection material and then calcining it once, mixing the calcined material with the iron phosphate synthesis mother liquor to prepare a slurry, and obtaining an anti-dissolved metal solution after solid-liquid separation; S2: mixing the reverse-dissolved metal solution with the ferrophosphorus slag acid-dissolved metal solution, adjusting the Fe / P molar ratio in the obtained mixed solution to (0.75-0.95):1, and the S / Fe molar ratio to (1-1.3):1, to obtain a mixed ferrophosphorus solution; S3: heating the mixed ferrophosphorus solution, adding a seed additive during the heating process, maintaining the temperature after the heating is completed to obtain ferrophosphate slurry, performing solid-liquid separation on the ferrophosphate slurry, and performing secondary roasting on the obtained solid phase to obtain anhydrous ferric phosphate.

2. The method according to claim 1, It is characterized in that In step S1, the iron phosphate dust collecting material includes anhydrous iron phosphate and dihydrate iron phosphate, and the sulfur content of the iron phosphate dust collecting material is 10000-20000 ppm.

3. The method according to claim 1, It is characterized in that In step S1, the pH of the ferric phosphate synthesis mother liquor is less than 1; and / or, during the mixed pulping process, the solid content of the pulp is controlled to be 10% to 25%.

4. The method according to claim 1, It is characterized in that In step S2, the reverse molten metal solution is mixed with the ferrophosphorus slag acid-soluble metal solution in a volume ratio of 1:4 to 1:2; the Fe / P molar ratio of the ferrophosphorus slag acid-soluble metal solution is (0.75-0.95):1, and the S / Fe molar ratio is (1-1.3):

1.

5. The method according to claim 1, It is characterized in that In step S2, the concentration of Fe in the mixed ferrophosphorus solution is 60-75 g / L.

6. The method according to claim 1, It is characterized in that In step S3, the heating process includes: heating to 85-95°C at a rate of 10°C / h-30°C / h, and then keeping the temperature for 10-20h.

7. The method according to claim 1, It is characterized in that In step S3, the seed additive is added when the temperature of the mixed ferrophosphorus solution reaches 50-60°C.

8. The method according to claim 1, It is characterized in that In step S3, the seed crystal additive is an iron phosphate slurry with a solid content of 20% to 40%; and / or the particle size D50 of the seed crystal additive is 1 to 1.5 μm.

9. The method according to claim 1, It is characterized in that In step S3, the mass of the seed additive is 5% to 20% of the mass of the mixed ferrophosphorus solution.

10. An iron phosphate, It is characterized in that The ferric phosphate is prepared by the method according to any one of claims 1 to 9, and the particle size D50 of the ferric phosphate is 3.5 to 6.5 μm.

Citation Information

Patent Citations

  • Method for treating waste lithium iron phosphate intermediate

    CN108929956A

  • Zero-discharge treatment system and process for iron phosphate wastewater

    CN115259516A

  • Recycling process of waste lithium iron phosphate battery

    CN116692910A

  • Method for preparing iron phosphate by recovering iron phosphate dust collecting material and application thereof

    CN117480117A