Composite sodium vanadium phosphate material, preparation method, application and energy storage device

By mixing sodium vanadium phosphate with metal sulfur carbide nanosheets and organic carbon source to prepare composite materials, the problems of poor conductivity and cyclic performance of sodium vanadium phosphate materials are solved, and the efficient electrochemical performance and long life of sodium ion batteries are achieved. , suitable for the positive electrode material of sodium ion batteries.

CN118929611AActive Publication Date: 2024-11-12BEIJING NADI TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411159395.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing sodium vanadium phosphate materials have low electronic conductivity, slow diffusion rate of sodium ions and poor water and oxygen stability, which limit the discharge rate and low temperature performance of sodium ion batteries, and have insufficient cycle life, making it difficult to be widely used in industrial applications.

Method used

By mixing sodium vanadium phosphate with metal sulfur carbide nanosheets and an organic carbon source for granulation and sintering, a composite sodium vanadium phosphate material with excellent electronic conductivity and electrochemical properties is prepared. The specific steps include the use of Nb2CSe2 or Ta2CSe2 nanosheets The ratio was adjusted to sodium vanadium phosphate and glucose, and metal sulfur carbide nanosheets were prepared by hydrothermal reaction or calcination and pickling, and sintered under the protection of inert gas after spray granulation.

Benefits of technology

It significantly improves the discharge specific capacity and cycling performance of composite vanadium phosphate materials, ensures efficient electrochemical performance, especially in high magnification and low temperature conditions, and is suitable for the positive electrode of sodium ion batteries. Material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929611A_ABST
    Figure CN118929611A_ABST
Patent Text Reader

Abstract

The invention discloses a composite sodium vanadium phosphate material, a preparation method, application and an energy storage device. The preparation method comprises the following steps: granulating and sintering a mixture containing sodium vanadium phosphate, metal thiocarbide nanosheets and an organic carbon source; the chemical formula of the metal thiocarbide nanosheet is M2CQ2, M is Nb and / or Ta, and Q is S and / or Se; the mass ratio of the sodium vanadium phosphate to the metal thiocarbide nanosheet is 100: (0.5-20), and the mass ratio of the sodium vanadium phosphate to the carbon source is 100: (2-30). The composite sodium vanadium phosphate material prepared by the invention has excellent electronic conductivity and electrochemical performance, and particularly has better specific discharge capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention specifically relates to a composite sodium vanadium phosphate material, a preparation method, an application and an energy storage device. Background Art

[0002] Sodium-ion batteries are considered to be a key new low-cost energy storage technology due to their advantages such as low raw material cost, excellent low-temperature performance, and good rate performance. The positive electrode material, as one of the most critical components of sodium-ion batteries, is the key to achieving long battery life, long life and high safety performance. Among them, sodium vanadium phosphate positive electrode material is designed as a positive electrode material with a long cycle life due to its stable structure, which can be used to greatly increase the service life of sodium-ion batteries and thus reduce the cost per kilowatt-hour. However, this material has obvious disadvantages: low electronic conductivity, slow sodium ion diffusion rate, and poor water and oxygen stability, so this type of material limits the discharge rate and low-temperature performance, and the electrode performance decays rapidly during the charge and discharge process. Although the preparation of sodium vanadium phosphate fluorophosphate positive electrode material by modifying sodium vanadium phosphate with fluorine can improve the charge and discharge potential and energy density, the problem of poor ion / electronic conductivity and cycle life is still difficult to solve. At present, there are few process technologies that fundamentally improve the electronic conductivity and rate characteristics of sodium vanadium phosphate positive electrode materials from the perspective of material structure design, which greatly limits the industrial application of sodium vanadium phosphate batteries. Summary of the invention

[0003] The technical problem solved by the present invention is to overcome the defects of poor conductivity and cycle performance of sodium vanadium phosphate materials in the prior art, and provide a composite sodium vanadium phosphate material and a preparation method, application and energy storage device. The composite sodium vanadium phosphate material prepared by the present invention has excellent electronic conductivity and electrochemical properties, especially has better discharge specific capacity and cycle performance.

[0004] The present invention solves the above technical problems through the following technical solutions:

[0005] The present invention provides a method for preparing a composite sodium vanadium phosphate material, which comprises the following steps: granulating and sintering a mixture containing sodium vanadium phosphate, metal sulfur carbide nanosheets and an organic carbon source to obtain the composite sodium vanadium phosphate material;

[0006] Among them, the chemical formula of the metal sulfide carbide nanosheets is M2CQ2, M is Nb and / or Ta, and Q is S and / or Se; the mass ratio of the sodium vanadium phosphate to the metal sulfide carbide nanosheets is 100:(0.5-20), and the mass ratio of the sodium vanadium phosphate to the carbon source is 100:(2-30).

[0007] In the present invention, the sodium vanadium phosphate preferably participates in the reaction in the form of particles.

[0008] In the present invention, the sodium vanadium phosphate can be obtained from conventional commercial sources or prepared by itself. The preparation method of the sodium vanadium phosphate preferably comprises the following steps: grinding a mixture of a sodium source and a vanadium source weighed in a stoichiometric ratio, and calcining the mixture at 400-900° C. for 2-12 hours under the protection of an inert gas.

[0009] Wherein, when the sodium source is NaH2PO4 and the vanadium source is vanadium pentoxide, the molar ratio of the sodium source to the vanadium source is 3:1.

[0010] The inert gas may be conventional in the art, such as nitrogen. The calcination temperature is preferably 600-800° C., such as 700° C. The calcination time is preferably 2-6 hours, such as 4 hours.

[0011] In the present invention, the metal sulfide carbide nanosheet is preferably one or more of Nb2CSe2, Ta2CSe2 and Nb2CS2, and more preferably Nb2CSe2 nanosheet. The sheet size of the metal sulfide carbide nanosheet can be 100nm-10μm, and the sheet thickness can be 5-20nm.

[0012] In the present invention, the method for preparing the metal carbide nanosheets preferably comprises the following steps:

[0013] Method 1: subjecting a hydrazine hydrate mixed solution containing metal sulfur carbide powder to a hydrothermal reaction to obtain the metal sulfur carbide nanosheets;

[0014] Alternatively, method 2: calcining and acid-washing a mixture of metal sulfide carbide powder and copper powder to obtain the metal sulfide carbide nanosheets.

[0015] The method for preparing the metal carbide powder preferably comprises the following steps: grinding and tabletting a mixture of a metal M source, a carbon source, a "sulfur source and / or a selenium source" and a catalyst weighed in a stoichiometric ratio, placing the mixture in a reaction tube, evacuating and sealing the reaction tube, and then calcining the mixture to obtain the powder.

[0016] The metal M source may be niobium powder and / or tantalum powder. The carbon source may be graphite. The sulfur source may be sulfur powder. The selenium source may be selenium powder. The catalyst may be one or more of hexachlorobenzene, chlorobenzene and benzene. The molar ratio of the metal M source, the carbon source, and the "sulfur source and / or selenium source" is, for example, 2:1:2. The mass of the catalyst is preferably 0.5%-10% of the total mass of the metal M source, the carbon source, and the "sulfur source and / or selenium source", for example 1%, 3%, 5%, 6% or 8%, more preferably 3%-8%.

[0017] The grinding operation and conditions can be conventional in the art, such as being carried out in a mortar. The tabletting equipment can be conventional in the art, such as a tablet press. The tabletting pressure is preferably 5-15 MPa, such as 10 MPa. The reaction tube is preferably a quartz tube. After the vacuuming, the vacuum degree of the reaction tube is preferably less than or equal to 10 -3 Pa. The sealing is generally performed by heating and melting both ends of the reaction tube. The calcination temperature is preferably 800-1400° C., such as 1200° C. The calcination time is preferably 2-8 hours, such as 5 hours.

[0018] Wherein, in method 1, the concentration of the hydrazine hydrate mixed solution containing metal sulfide carbide powder is preferably 30-80 mg / mL, for example, 50 mg / mL. The concentration refers to the ratio of the mass of the metal sulfide carbide powder to the volume of the hydrazine hydrate mixed solution containing the metal sulfide carbide powder. In the hydrazine hydrate mixed solution containing the metal sulfide carbide powder, the solvent is generally a mixture of hydrazine hydrate aqueous solution and deionized water. The volume ratio of the hydrazine hydrate aqueous solution to deionized water can be 1:(2-5), for example, 1:3.

[0019] Among them, in method 1, the hydrothermal reaction is generally carried out in a reactor. The temperature of the hydrothermal reaction can be 90-140°C, such as 120°C. The time of the hydrothermal reaction can be 12-48h, such as 18h, 24h or 30h. According to the convention in the art, after the hydrothermal reaction is completed, washing and drying are generally required.

[0020] Wherein, in method 2, the molar ratio of the metal carbide powder to the copper powder may be 1:(0.5-2), for example, 1:1 or 1:1.5. The mixture generally needs to be ground before calcining. The calcination is generally carried out under an inert atmosphere, such as nitrogen. The calcination temperature is preferably 500-1000°C, for example, 600°C, 800°C or 900°C. The calcination time is preferably 2-8h, for example, 4h. The acid used for the pickling is preferably concentrated hydrochloric acid. The concentration of the concentrated hydrochloric acid is, for example, 12M. The pickling time may be 2-8h, for example, 6h. The pickling is generally carried out under stirring. The stirring speed may be 200-600rpm, for example, 300rpm. After the pickling is completed, washing and drying are generally required.

[0021] In order to better maintain the dispersed state of the nanosheets, the metal carbide sulfide nanosheets are generally prepared into a dispersion for storage.

[0022] In the present invention, the organic carbon source may be one or more of glucose, sucrose, fructose and starch, preferably glucose and / or sucrose.

[0023] In the present invention, the mass ratio of the sodium vanadium phosphate to the metal sulfur carbide nanosheets is preferably 100:(0.5-10), for example, 100:1, 100:3, 100:4, 100:5, 100:6 or 100:10.

[0024] In the present invention, the mass ratio of the sodium vanadium phosphate to the carbon source is preferably 100:(2-20), for example, 100:5, 100:8, 100:10, 100:15 or 100:20.

[0025] In the present invention, the sodium vanadium phosphate, the metal sulfide carbide nanosheets and the organic carbon source are preferably mixed before the granulation. The mixing speed may be 500-2000 rpm, such as 1500 rpm. The mixing time may be 10-60 min, such as 30 min.

[0026] In the present invention, a small amount of solvent is generally required to be added before granulation. For example, the sodium vanadium phosphate, the metal sulfide carbide nanosheets, the organic carbon source and the solvent can be mixed before granulation; or one or more of the sodium vanadium phosphate, the metal sulfide carbide nanosheets and the organic carbon source can be added to the reaction system in the form of a dispersion.

[0027] In the present invention, the metal sulfide carbide nanosheets are preferably added to the reaction system in the form of a metal sulfide carbide nanosheet dispersion. The concentration of the metal sulfide carbide nanosheet dispersion is preferably 0.5-5 mg / mL, such as 1 mg / mL or 2 mg / mL. The concentration refers to the ratio of the mass of the metal sulfide carbide nanosheets to the volume of the metal sulfide carbide nanosheet dispersion. In the metal sulfide carbide nanosheet dispersion, the solvent can be one or more of ethanol, methanol and deionized water, such as ethanol.

[0028] In the present invention, the granulation method is preferably spray granulation. The spray granulation is generally performed in a spray granulator. The process parameters of the spray granulation can be an air inlet temperature of 170-220°C (e.g. 190°C) and an air outlet temperature of 80-110°C (e.g. 95°C).

[0029] In the present invention, the sintering is generally carried out under the protection of an inert gas. The sintering temperature may be 400-800° C., such as 450° C., 500° C., 550° C. or 600° C., preferably 500-700° C. The sintering time may be 1-6 hours, such as 2 hours, 3 hours or 4 hours, preferably 1-3 hours.

[0030] The present invention also provides a composite sodium vanadium phosphate material prepared by the above-mentioned preparation method.

[0031] In the present invention, the shape of the composite sodium vanadium phosphate material can be spherical or quasi-spherical. The size of the composite sodium vanadium phosphate material can be 5nm-50μm, preferably 50nm-20μm.

[0032] The present invention also provides an application of the composite sodium vanadium phosphate material as described above in a sodium ion battery. Preferably, the composite sodium vanadium phosphate material is used as a positive electrode material.

[0033] The present invention also provides an energy storage device, which comprises the composite sodium vanadium phosphate material as described above.

[0034] Wherein, the energy storage device is preferably a sodium ion secondary battery, a sodium ion capacitor, a sodium-air battery, a sodium-sulfur battery or a derivative energy storage device.

[0035] The raw materials and reagents used in the present invention are commercially available.

[0036] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0037] The reagents and raw materials used in the present invention are commercially available.

[0038] The positive and progressive effects of the present invention are:

[0039] (1) The method of the present invention has a simple synthesis process and high raw material utilization rate, which is conducive to industrial production;

[0040] (2) The composite sodium vanadium phosphate material prepared by the present invention has excellent electronic conductivity and electrochemical properties, especially better discharge specific capacity and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the SEM image of the Nb2CSe2 nanosheets prepared in Example 1;

[0042] Figure 2 This is a SEM image of the composite sodium vanadium phosphate material prepared in Example 1;

[0043] Figure 3 This is the XRD pattern of the Nb2CSe2 powder prepared in Example 1;

[0044] Figure 4 is the xrd diagram of Ta2CSe2 powder prepared in Example 8;

[0045] Figure 5 This is the XRD diagram of the Nb2CS2 powder prepared in Example 9;

[0046] Figure 6 This is the XRD diagram of Ta2CS2 powder prepared in Example 10. DETAILED DESCRIPTION

[0047] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0048] Example 1

[0049] (1) vanadium pentoxide and NaH2PO4 are fully ground and mixed in a molar ratio of 1:3, and then placed in a tube furnace, heated to 700°C at a heating rate of 5°C / min under nitrogen atmosphere and kept at this temperature for 4 hours, and then cooled to obtain sodium vanadium phosphate particles;

[0050] (2) Weigh niobium powder, graphite powder and selenium powder in a molar ratio of 2:1:2, add hexachlorobenzene (6% of the total weight of the niobium powder, graphite powder and selenium powder), grind them evenly with a mortar, press them into thin sheets with a tablet press at a pressure of 10 MPa, place them in a quartz tube, evacuate the quartz tube and seal it with a hydrogen-oxygen flame gun (vacuum degree less than 10 -3 Pa), transferred to a muffle furnace for calcination, the heating rate was 5 ° C / min, the calcination temperature was 1200 ° C, the calcination time was 5 h, and Nb2CSe2 powder was obtained after cooling;

[0051] Preparation of Nb2CSe2 nanosheets: Weigh Nb2CSe2 powder to prepare a mixed solution with a concentration of 50 mg / mL, the solvent is a mixed solution of hydrazine hydrate solution and deionized water (the volume ratio of hydrazine hydrate solution to deionized water is 1:3, and the hydrazine hydrate solution is purchased from Aladdin), transfer to a reactor for hydrothermal reaction at 120°C for 24 hours, cool, filter, wash, and dry to obtain intercalated Nb2CSe2 nanosheets; disperse the Nb2CSe2 nanosheets in ethanol to prepare a 1 mg / mL Nb2CSe2 nanosheet dispersion;

[0052] (3) Sodium vanadium phosphate, Nb2CSe2 nanosheet dispersion and glucose are placed in a high-speed mixer and mixed at 1500 rpm for 30 minutes to obtain a precursor slurry; the precursor slurry is pumped into a spray granulator and spray granulated at an air inlet temperature of 190°C and an air outlet temperature of 95°C. After granulation, the mixture is transferred to a tubular furnace and sintered under a nitrogen atmosphere at a temperature of 600°C for 2 hours. After sintering, the mixture is naturally cooled to room temperature to obtain a composite sodium vanadium phosphate material; wherein the mass ratio of sodium vanadium phosphate to Nb2CSe2 nanosheets in the Nb2CSe2 nanosheet dispersion is 100:1, and the mass ratio of sodium vanadium phosphate to glucose is 100:10.

[0053] Example 2

[0054] Compared with Example 1, except that the mass ratio of sodium vanadium phosphate to Nb2CSe2 nanosheets in step (3) is replaced with 100:3, the other parameters and conditions are the same as those in Example 1.

[0055] Example 3

[0056] Compared with Example 1, except that the mass ratio of sodium vanadium phosphate to Nb2CSe2 nanosheets in step (3) is replaced with 100:5, the other parameters and conditions are the same as those in Example 1.

[0057] Example 4

[0058] Compared with Example 1, except that the mass ratio of sodium vanadium phosphate to Nb2CSe2 nanosheets in step (3) is replaced with 100:10, the other parameters and conditions are the same as those in Example 1.

[0059] Example 5

[0060] Compared with Example 1, except that the mass ratio of sodium vanadium phosphate to glucose in step (3) is replaced with 100:5, the other parameters and conditions are the same as those in Example 1.

[0061] Example 6

[0062] Compared with Example 1, except that the mass ratio of sodium vanadium phosphate to glucose in step (3) is replaced with 100:20, the other parameters and conditions are the same as those in Example 1.

[0063] Example 7

[0064] (1) Same as Example 1;

[0065] (2) Preparation of Nb2CSe2 powder is the same as in Example 1;

[0066] Preparation of Nb2CSe2 nanosheets: grind and mix Nb2CSe2 powder and high-purity copper powder in a molar ratio of 1:1, put into a tube furnace, heat to 800°C at a heating rate of 5°C / min under nitrogen atmosphere and keep warm for 4 hours, cool and put into excess 12M concentrated hydrochloric acid and stir at 300rpm for 6 hours, filter, wash three times with water and ethanol, and dry to obtain intercalated Nb2CSe2 nanosheets; disperse Nb2CSe2 nanosheets in ethanol to prepare 1 mg / mL Nb2CSe2 nanosheet dispersion;

[0067] (3) As in Example 1, a composite sodium vanadium phosphate positive electrode material was prepared.

[0068] Example 8

[0069] (1) Same as Example 1;

[0070] (2) The niobium powder was replaced with tantalum powder, and the other aspects were the same as in Example 1 to obtain Ta2CSe2;

[0071] (3) Except for replacing Nb2CSe2 with Ta2CSe2 prepared in step (2), the other steps are the same as in Example 1 to obtain a composite sodium vanadium phosphate positive electrode material.

[0072] Example 9

[0073] (1) Same as Example 1;

[0074] (2) Selenium powder was replaced with sulfur powder, and the other aspects were the same as in Example 1 to obtain Nb2CS2;

[0075] (3) Except for replacing Nb2CSe2 with Nb2CS2 prepared in step (2), the other steps are the same as in Example 1 to obtain a composite sodium vanadium phosphate positive electrode material.

[0076] Example 10

[0077] (1) Same as Example 1;

[0078] (2) The niobium powder was replaced by tantalum powder, the selenium powder was replaced by sulfur powder, and the rest was the same as in Example 1 to obtain Ta2CS2;

[0079] (3) Except for replacing Nb2CSe2 with Ta2CS2 prepared in step (2), the other steps are the same as in Example 1 to obtain a composite sodium vanadium phosphate positive electrode material.

[0080] Embodiment 11

[0081] Compared with Example 1, except that the hexachlorobenzene added in step (2) is adjusted from 6% to 1% of the solid mass, the other parameters and conditions are the same as those in Example 1.

[0082] Example 12

[0083] Compared with Example 1, except that the hexachlorobenzene in step (2) is replaced by chlorobenzene, the other parameters and conditions are the same as those in Example 1.

[0084] Example 13

[0085] Compared with Example 1, except that the glucose in step (3) is replaced by sucrose, the other parameters and conditions are the same as those in Example 1.

[0086] Embodiment 14

[0087] Compared with Example 1, except that the sintering temperature in step (3) is adjusted to 450° C., the other parameters and conditions are the same as those in Example 1.

[0088] Embodiment 15

[0089] Compared with Example 1, except that the sintering time in step (3) is adjusted to 4 hours, the other parameters and conditions are the same as those in Example 1.

[0090] Comparative Example 1

[0091] The sodium vanadium phosphate material prepared in step (1) in Example 1.

[0092] Comparative Example 2

[0093] Compared with Example 1, except for eliminating the addition of Nb2CSe2 nanosheets in step (3), the rest is the same as Example 1.

[0094] Comparative Example 3

[0095] Compared with Example 1, except for eliminating the addition of glucose in step (3), the rest is the same as Example 1.

[0096] Effect Example

[0097] (1) Morphological characterization

[0098] Figure 1 This is a SEM image of the Nb2CSe2 nanosheet prepared in Example 1, showing that it is a sheet-like nano-agglomerate structure, with a sheet size ranging from 200 nanometers to 5 micrometers and a thickness of about 10 nanometers; Figure 2 This is a SEM image of the composite sodium vanadium phosphate material prepared in Example 1. After mixing and granulation, spherical particles with a diameter of 1 micron to 20 microns were obtained.

[0099] (2) Electrochemical performance test

[0100] The positive electrode materials prepared in Examples 1-15 and Comparative Examples 1-3 were applied to button batteries for electrochemical performance testing. The battery assembly process was as follows:

[0101] The positive electrode material, polyvinylidene fluoride (PVDF) and conductive carbon black were mixed in a mass ratio of 8:1:1 and dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry. The slurry was evenly coated on aluminum foil to prepare a positive electrode sheet. The coated electrode sheet was placed in a vacuum drying oven at a temperature of 120°C and vacuum dried for 12 hours. The electrode sheet was taken out and cut into a circular electrode sheet with a diameter of 12 mm using a cutting machine. The loading amount of active material on the positive electrode sheet was 3 mg / cm 2 ;

[0102] When assembling the battery, a glass fiber diaphragm from Whatman was used; the electrolyte was 1M NaPF6 electrolyte, the solvent was EC (ethylene carbonate) and DMC (dimethyl carbonate), the volume ratio of EC: DMC = 1:1, and the metal sodium sheet was the counter electrode; finally, the positive electrode sheet, sodium sheet, spring, gasket, positive electrode shell, negative electrode shell, diaphragm, and electrolyte were assembled into a CR2025 button half-cell in an argon-filled glove box. The charge and discharge voltage range is 2.0-4.1V, the first charge and discharge rate is 0.1C, and the nominal specific capacity is 1C = 100mAh / g. The charge and discharge rate of the cycle performance test is 1C cycle 300 weeks. The test results are shown in Table 1:

[0103] Table 1

[0104]

[0105]

[0106] According to the above experimental results, the composite sodium vanadium phosphate positive electrode material prepared by the present invention has excellent electrochemical properties, with a 1C discharge specific capacity of more than 105 mAh / g, a 10C discharge specific capacity of more than 92 mAh / g, and an energy retention rate of more than 88% after 1000 cycles.

[0107] According to Example 1 and Comparative Examples 1-3, when only sodium vanadium phosphate is used without adding metal sulfur carbide nanosheets or organic carbon source, the 1C discharge specific capacity and the 10C discharge specific capacity are both reduced, especially after 1000 cycles, the energy retention rate is even as low as 73%.

[0108] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.

Claims

1. A method for preparing a composite sodium vanadium phosphate material, It is characterized in that The method comprises the following steps: granulating and sintering a mixture containing sodium vanadium phosphate, metal sulfur carbide nanosheets and an organic carbon source to obtain the composite sodium vanadium phosphate material; Wherein, the chemical formula of the metal carbide nanosheet is M 2 CQ 2 , M is Nb and / or Ta, Q is S and / or Se; the mass ratio of the sodium vanadium phosphate to the metal sulfur carbide nanosheets is 100:(0.5-20), and the mass ratio of the sodium vanadium phosphate to the carbon source is 100:(2-30).

2. The method for preparing the composite sodium vanadium phosphate material according to claim 1, It is characterized in that The preparation method meets one or more of the following conditions: (1) The preparation method of sodium vanadium phosphate comprises the following steps: grinding a mixture of a sodium source and a vanadium source weighed in a stoichiometric ratio, and calcining at 400-900° C. for 2-12 hours under the protection of an inert gas; (2) The metal sulfide carbide nanosheet is Nb 2 CSe 2 、 2 CSe 2 and Nb 2 CS 2 One or more of, preferably Nb 2 CSe 2 Nanosheets; (3) The sheet size of the metal carbide nanosheet is 100 nm-10 μm, and the sheet thickness is 5-20 nm; (4) The organic carbon source is one or more of glucose, sucrose, fructose and starch, preferably glucose and / or sucrose.

3. The method for preparing the composite sodium vanadium phosphate material according to claim 1, It is characterized in that The preparation method meets one or more of the following conditions: (1) the metal sulfide carbide nanosheets are added to the reaction system in the form of a metal sulfide carbide nanosheet dispersion; The concentration of the metal carbide sulfide nanosheet dispersion is preferably 0.5-5 mg / mL; In the metal carbide sulfide nanosheet dispersion, the solvent is preferably one or more of ethanol, methanol and deionized water; (2) The mass ratio of the sodium vanadium phosphate to the metal sulfur carbide nanosheets is 100:(0.5-10), for example, 100:1, 100:3, 100:4, 100:5, 100:6 or 100:10; (3) The mass ratio of the sodium vanadium phosphate to the carbon source is 100:(2-20), for example, 100:5, 100:8, 100:10, 100:15 or 100:20; (4) before granulation, sodium vanadium phosphate, metal sulfur carbide nanosheets and an organic carbon source are mixed; (5) The process parameters of the spray granulation are an air inlet temperature of 170-220°C and an air outlet temperature of 80-110°C; (6) The sintering temperature is 400-800°C, such as 450°C, 500°C, 550°C or 600°C, preferably 500-700°C; (7) The sintering time is 1-6 hours, such as 2 hours, 3 hours or 4 hours, preferably 1-3 hours.

4. The method for preparing the composite sodium vanadium phosphate material according to claim 1, It is characterized in that The method for preparing the metal carbide nanosheets comprises the following steps: Method 1: subjecting a hydrazine hydrate mixed solution containing metal sulfur carbide powder to a hydrothermal reaction to obtain the metal sulfur carbide nanosheets; Alternatively, method 2: calcining and acid-washing a mixture of metal sulfide carbide powder and copper powder to obtain the metal sulfide carbide nanosheets.

5. The method for preparing the composite sodium vanadium phosphate material according to claim 4, It is characterized in that The preparation method of the metal sulfur carbide powder comprises the following steps: grinding and tableting a mixture of a metal M source, a carbon source, a "sulfur source and / or a selenium source" and a catalyst weighed in a stoichiometric ratio, placing the mixture in a reaction tube, evacuating and sealing the reaction tube, and calcining the mixture to obtain the metal sulfur carbide powder; The mass of the catalyst is preferably 0.5%-10% of the total mass of the metal M source, the carbon source, and the "sulfur source and / or selenium source", for example 1%, 3%, 5%, 6% or 8%, more preferably 3%-8%; The calcination temperature is preferably 800-1400° C., such as 1200° C.; the calcination time is preferably 2-8 h, such as 5 h.

6. The method for preparing the composite sodium vanadium phosphate material according to claim 4, It is characterized in that The method 1 satisfies one or more of the following conditions: (1) The concentration of the hydrazine hydrate mixed solution containing metal sulfur carbide powder is 30-80 mg / mL; (2) In the hydrazine hydrate mixed solution containing metal sulfur carbide powder, the solvent is a mixed solution of hydrazine hydrate aqueous solution and deionized water; The volume ratio of the hydrazine hydrate aqueous solution to deionized water is preferably 1:(2-5); (3) The temperature of the hydrothermal reaction is 90-140° C.; (4) The hydrothermal reaction time is 12-48h.

7. The method for preparing the composite sodium vanadium phosphate material according to claim 4, It is characterized in that The second method meets one or more of the following conditions: (1) The molar ratio of the metal carbide powder to the copper powder is 1:(0.5-2); (2) The calcination temperature is 500-1000° C.; (3) The calcination time is 2-8h; (4) The acid used in the pickling is concentrated hydrochloric acid; (5) The pickling time is 2-8 hours.

8. A composite sodium vanadium phosphate material, It is characterized in that The composite sodium vanadium phosphate material is prepared according to the preparation method of the composite sodium vanadium phosphate material according to any one of claims 1 to 7.

9. Use of the composite sodium vanadium phosphate material as claimed in claim 8 in a sodium ion battery.

10. An energy storage device, It is characterized in that It includes the composite sodium vanadium phosphate material as described above; The energy storage device is preferably a sodium ion secondary battery, a sodium ion capacitor, a sodium-air battery, a sodium-sulfur battery or a derivative energy storage device.

Citation Information

Patent Citations

  • Sodium vanadium phosphate composite cathode material and preparation method thereof

    CN111994890A

  • Oxide-coated sodium battery positive electrode material as well as preparation method and application thereof

    CN115425196A

  • Double-carbon-layer heterogeneous composite positive electrode material, preparation thereof and sodium ion battery

    CN116741975A

  • Alkali metal or Alkali-Ion batteries having high volumetric and gravimetric energy densities

    US20170077546A1