Preparation method of high-porosity foamy carbon for silicon carbide crystal growth
By preparing high-porosity foamed carbon as a substitute for porous graphite, the problems of low porosity and easy corrosion of porous graphite in the silicon carbide crystal growth process were solved, realizing efficient silicon carbide crystal growth and reducing production costs.
Patent Information
- Application Number
- CN202410989056.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing porous graphite has problems such as low porosity, few through-holes, high cost, complex process, and easy corrosion in silicon carbide crystal growth, which affect the quality of silicon carbide crystals and production efficiency.
Synthetic sponge was used as a porous template, and the template strength was enhanced by carbon precursor solution to prepare high-porosity foam carbon. A two-stage carbonization process was carried out in an Ar atmosphere, and the heating rate and gas flow rate were controlled to remove organic matter, resulting in high-porosity foam carbon with three-dimensional interconnected channels.
The prepared high-porosity foam carbon has a porosity of over 80% and good mechanical strength, which can effectively replace porous graphite, improve gas mass transfer efficiency, improve the crystallization quality of silicon carbide crystals, and reduce production costs.
Smart Images

Figure CN118929625A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a method for preparing high-porosity foamed carbon. Background Art
[0002] In recent years, silicon carbide has shown great application potential due to its wide bandgap, high breakdown field strength, high thermal conductivity and many other characteristics. In particular, with the application of silicon carbide devices in the field of electric vehicles, the silicon carbide industry has received widespread attention from all walks of life.
[0003] There are many methods for growing silicon carbide single crystals, such as the liquid phase method, the PVT method, and the HTCVD method. However, the only commercially available method for producing silicon carbide single crystals is the physical vapor transport method, or PVT method. The PVT method is usually as follows: silicon carbide raw materials are placed at the bottom of the crucible, and silicon carbide seed crystals are placed at the top. The crucible has a certain axial and radial temperature gradient through the design of the insulation structure. The crucible is heated to 2000℃~2400℃ to evaporate and sublimate the silicon carbide raw materials to form a gas phase. Under the action of the temperature gradient, the gas phase is transported from the bottom of the crucible to the seed crystal for crystallization, thereby growing a silicon carbide single crystal.
[0004] The crystal quality and yield of silicon carbide directly determine its core competitiveness, among which carbon coating is a major factor affecting the quality of silicon carbide crystals. The main source of carbon coating is: in the PVT crystal growth process, carbon particles after powder sublimation or carbon particles after crucible corrosion are carried to the surface of the ingot by airflow under the action of temperature gradient, and enter the crystal to form defects.
[0005] In order to reduce the generation of carbon encapsulation, a piece of porous graphite can usually be set in the mass transfer path of the gas to filter the carbon particles in the atmosphere, and it can also play a role in the uniform flow redistribution of the mass transfer gas flow. However, there are still many problems in the application of porous graphite in the field of silicon carbide crystal growth: first, the production cycle of porous graphite is long and the production capacity is low. Only a few companies such as SGL, Morgan, and Semik can provide qualified porous graphite at home and abroad; second, porous graphite is mostly sintered after adding pore-forming agents to graphite particles, which is also one of the sources of carbon particles at high temperatures. The process is complicated and the cost is high, which is not conducive to large-scale application; third, due to process problems, it is difficult to obtain porous graphite with high porosity and high through-porosity. The porosity of common porous graphite is about 50%, and the through-porosity is even halved, which greatly affects the application of porous graphite. Therefore, the industry urgently needs a high-porosity carbon material to replace porous graphite. Summary of the invention
[0006] In view of the above problems, the present invention provides a method for preparing high-porosity foam carbon for silicon carbide crystal growth, which has the advantages of simple process, fast production cycle, low cost, etc. The porosity can reach more than 80%, and basically all of them are through holes, and the comprehensive performance is better than porous graphite.
[0007] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0008] A method for preparing high-porosity foamed carbon for silicon carbide crystal growth comprises the following steps:
[0009] (1) Clean the synthetic sponge and dry it at low temperature;
[0010] (2) immersing the dried synthetic sponge in the carbon precursor solution, taking it out after it is completely soaked, and drying and curing it to obtain a foamed carbon precursor;
[0011] (3) placing the carbon foam precursor into a high-temperature furnace for heating and carbonization to obtain high-porosity carbon foam.
[0012] According to the above scheme, the synthetic sponge used in step 1 is polyurethane sponge or polyvinyl alcohol sponge.
[0013] According to the above scheme, the porosity of the synthetic sponge used in step 1 is above 90%, and the pore size is between 10ppi and 100ppi.
[0014] According to the above scheme, step 1 is cleaned with deionized water, anhydrous ethanol or isopropanol; and the drying temperature is not higher than 100°C.
[0015] According to the above scheme, the mass concentration of the organic resin in the carbon precursor solution in step 2 is 15% to 50%.
[0016] According to the above scheme, the carbon precursor solution in step 2 is a solution of an organic resin; the resin is one or any combination of phenolic resin, furfural resin, and benzoxazine; and the solvent is ethanol, acetone or deionized water.
[0017] According to the above scheme, the drying and curing temperature in step 2 is 80 to 200° C., and the curing time is 5 to 20 hours.
[0018] In the optimized solution, the synthetic sponge is a polyurethane sponge; the carbon precursor solution is a benzoxazine resin solution, and the mass concentration of the resin is 20-40%.
[0019] According to the above scheme, the carbonization process in step 3 is carried out in two stages; the first stage is kept warm at three temperature ranges of 100-200°C, 400-550°C, and 700-1200°C at a heating rate of 0.5-5°C / min for 1-5h; the second stage is kept warm at 2000-2300°C at a heating rate of 5-10°C / min for 1-10h.
[0020] According to the above scheme, the carbonization process in step 3 is carried out in an Ar gas atmosphere, the pressure in the high-temperature furnace is 10 to 80 kPa, and the Ar gas flow rate is 5 to 20 SLM.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] Since Si vapor exists in the atmosphere during the silicon carbide crystal growth process, it is easy to corrode graphite, especially porous graphite, causing it to lose mechanical properties, bend or break, and seriously affect the temperature field and flow field. Conventional porous graphite not only has low porosity and few through holes, but also has relatively weak material mechanical strength. The high-porosity foamed carbon prepared by the present invention not only has a porosity of more than 80% and almost all through holes, but also has good material mechanical strength. It is not easy to bend or break when used, and can effectively replace porous graphite and expand its application range.
[0023] Taking artificial synthetic sponge as a porous template, relying on the rich three-dimensional pore structure of the sponge, the strength of the template is enhanced by a carbon precursor solution to obtain a high-porosity foam carbon with three-dimensional through holes. The first carbonization process of the synthetic sponge mainly plays the role of negative pressure degreasing and preliminary carbonization. Since the synthetic sponge and the carbon precursor solution are both high-molecular organic compounds, a large amount of organic matter and gas will be released during the carbonization process, which is very easy to contaminate the sample or cause equipment blockage. The use of negative pressure and a large gas flow rate in this carbonization process can effectively remove organic matter and gas, maintain the surface cleanliness of the foam carbon, and perform preliminary carbonization on the foam carbon. In the second carbonization process, the carbonization of the foam carbon is more thorough, the residual organic matter in the first carbonization process is further decomposed, and the amorphous carbon converted from the carbon precursor solution is graphitized more deeply with the increase of temperature, and the overall structural strength of the foam carbon is improved.
[0024] The present invention can obtain high-porosity foamed carbon with a porosity of more than 80% and good mechanical strength. The foamed carbon is used for silicon carbide crystal growth, which can effectively improve gas mass transfer efficiency and improve crystallization. The foamed carbon has a three-dimensionally connected pore structure and does not have a small particle carbon source of porous graphite, so it is not only conducive to improving gas mass transfer, but also can avoid becoming a source of carbon encapsulation, and can effectively improve the crystallization quality of silicon carbide crystals. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 : The present invention is a process flow chart for preparing high-porosity foamed carbon for silicon carbide crystal growth.
[0026] Figure 2 : Microscopic morphology of the high-porosity foam carbon prepared in Example 1 for silicon carbide crystal growth.
[0027] Figure 3 : Microscopic morphology of the high-porosity foam carbon prepared in Example 2 for silicon carbide crystal growth.
[0028] Figure 4 : Microscopic morphology of the high-porosity foam carbon prepared in Example 3 for silicon carbide crystal growth.
[0029] Figure 5 : Defect distribution diagram of silicon carbide crystal obtained using porous graphite.
[0030] Figure 6 : Defect distribution diagram of silicon carbide crystal obtained using the high-porosity foam carbon obtained in Example 1. DETAILED DESCRIPTION
[0031] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0032] The specific embodiment provides a method for preparing high-porosity foamed carbon for silicon carbide crystal growth. The process flow chart is shown in the attached Figure 1 As shown:
[0033] (1) Cleaning the synthetic sponge and drying it at low temperature; the synthetic sponge is a polyurethane sponge or a polyvinyl alcohol sponge; the porosity is above 90% and the pore size is between 10 ppi and 100 ppi;
[0034] (2) immersing the dried synthetic sponge in a carbon precursor solution, taking it out after it is completely soaked, drying and curing it to obtain a foamed carbon precursor; the carbon precursor solution is one or any combination of phenolic resin, furfural resin, and benzoxazine; the drying and curing temperature is 80 to 200° C., and the curing time is 5 to 20 hours;
[0035] (3) placing the foamed carbon precursor into a high-temperature furnace and heating it in an Ar gas atmosphere for carbonization, wherein the pressure in the high-temperature furnace is 10 to 80 kPa and the Ar gas flow rate is 5 to 20 SLM; obtaining a high-porosity foamed carbon; the carbonization process is carried out in two stages; in the first stage, the temperature is kept at 100 to 200 ° C, 400 to 550 ° C, and 700 to 1200 ° C at a heating rate of 0.5 to 5 ° C / min for 1 to 5 h; in the second stage, the temperature is kept at 2000 to 2300 ° C at a heating rate of 5 to 10 ° C / min for 1 to 10 h.
[0036] Polyvinyl alcohol sponge, purchased from Lishui Yunchuang Sponge Products Co., Ltd., with a pore size of 40PPi. Phenolic resin, purchased from Henan Zhongfan Dongsheng New Materials Technology Co., Ltd., with a molecular weight of 120-200. Polyurethane sponge, purchased from Kunshan Yuanshengxing New Materials Co., Ltd., with a pore size of 60ppi. Benzoxazine resin, purchased from Jining Ribushi Biotechnology Co., Ltd., with a molecular weight of 200-400. Furfural resin solution, purchased from Hubei Langbowan Biomedicine Co., Ltd., with a molecular weight of 1000-3000. The rest of the raw materials not mentioned in the preparation were obtained from conventional commercial channels unless otherwise specified.
[0037] Example 1
[0038] (1) Use a polyvinyl alcohol sponge with a pore size of 40 PPi, clean it with anhydrous ethanol, and dry it in an oven at 80°C.
[0039] (2) A phenolic resin solution with a mass concentration of 40% was prepared, and the solvent was anhydrous ethanol. The polyvinyl alcohol sponge was completely soaked in the phenolic resin solution, then taken out and placed in an oven at 150° C. for curing for 10 h.
[0040] (3) The cured polyvinyl alcohol sponge was placed in a high-temperature furnace, and after evacuation, the pressure was filled to 20 kPa with an Ar flow rate of 5 SLM and maintained, and then the temperature was increased at a rate of 2 °C / min, and kept at 120 °C, 400 °C, and 900 °C for 2 h, respectively, to obtain a preliminary degreased carbonized foam carbon.
[0041] (4) The carbon foam obtained in (3) was placed back in the high-temperature furnace, and after evacuation, the furnace was pressurized to 20 kPa with an Ar flow rate of 5 SLM and maintained, and the temperature was raised to 2000°C at a rate of 5°C / min and kept at this temperature for 3 h to obtain a completely carbonized carbon foam with high porosity.
[0042] The microscopic morphology of the high porosity foamed carbon obtained in this example is shown in the attached Figure 2 shown.
[0043] Example 2
[0044] (1) Select a polyurethane sponge with a pore size of 60 ppi, clean it with deionized water, and dry it in an oven at 50°C.
[0045] (2) A benzoxazine resin solution with a mass concentration of 30% was prepared, and the solvent was deionized water. The polyurethane sponge was completely soaked in the benzoxazine resin solution, then taken out and placed in an oven at 130° C. for curing for 8 h.
[0046] (3) The cured polyurethane sponge was placed in a high-temperature furnace, and after evacuation, the pressure was filled to 30 kPa at an Ar flow rate of 10 SLM and maintained, and then the temperature was increased at a rate of 0.5 °C / min, and kept at 210 °C, 500 °C, and 1100 °C for 3 h, respectively, to obtain preliminary degreased carbonized foam carbon.
[0047] (4) The carbon foam obtained in (3) was placed back in a high-temperature furnace, and after evacuation, the furnace was pressurized to 30 kPa with an Ar flow rate of 10 SLM and maintained, and then the temperature was increased to 2200 °C at a rate of 10 °C / min and kept at this temperature for 2 h to obtain a completely carbonized carbon foam with high porosity.
[0048] The microscopic morphology of the high porosity foamed carbon obtained in this example is shown in the attached Figure 3 shown.
[0049] Example 3
[0050] (1) Select a polyurethane sponge with a pore size of 60 ppi, clean it with anhydrous ethanol, and dry it in an oven at 50°C.
[0051] (2) A furfural resin solution with a mass concentration of 25% was prepared, and the solvent was acetone. The polyurethane sponge was completely soaked in the furfural resin solution, then taken out and placed in an oven at 90° C. for curing for 15 h.
[0052] (3) The cured polyurethane sponge was placed in a high-temperature furnace, and after evacuation, the pressure was filled to 60 kPa with an Ar flow rate of 10 SLM and maintained, and then the temperature was increased at a rate of 1 °C / min, and kept at 150 °C, 500 °C, and 1000 °C for 1 h, respectively, to obtain preliminary degreased carbonized foam carbon.
[0053] (4) The carbon foam obtained in (3) was placed back in a high-temperature furnace, and after evacuation, the furnace was pressurized to 60 kPa with an Ar flow rate of 10 SLM and maintained, and then the temperature was increased to 2300 °C at a rate of 5 °C / min and kept at that temperature for 1 h to obtain a completely carbonized carbon foam with high porosity.
[0054] The microscopic morphology of the high porosity foamed carbon obtained in this example is shown in the attached Figure 4 shown.
[0055] The mechanical strength and porosity of the foamed carbon and domestic porous graphite prepared in Example 1, Example 2, and Example 3 are shown in Table 1. The foamed carbon prepared by the present invention has relatively better mechanical strength and porosity. This is because the resin is a polymer compound, and the molecules are relatively continuous after carbonization, and there will be a certain degree of shrinkage during carbonization, which further improves the strength of the matrix. Among them, benzoxazine, as a new type of resin that has just emerged in recent years, produces almost no gas during curing, so it is not easy to produce defects such as pores inside the matrix pores, and therefore has stronger mechanical strength. Relying on the three-dimensional pore structure of the synthetic sponge, the foamed carbon made therefrom also has a larger porosity.
[0056]
[0057] The porous foam carbon prepared in Example 2 and the domestic porous graphite were selected for comparison of silicon carbide crystal growth experiments. Both experiments were carried out in an induction crystal growth furnace, and the crystal growth process was: growth temperature 2200°C, furnace pressure 7mbar, growth time 120h, and the growth process was carried out in an Ar gas atmosphere.
[0058] Defects of silicon carbide grown using domestic porous graphite Figure 5 The defect diagram of silicon carbide grown after using the porous foam carbon prepared in Example 2 of the present invention is shown in FIG. Figure 6 As shown, by comparison, it can be seen that after using the porous foam carbon prepared by the present invention, the number of defects in the silicon carbide crystal is significantly reduced.
Claims
1. A method for preparing high-porosity foamed carbon for silicon carbide crystal growth, Features The following steps are involved: (1) Clean the synthetic sponge and dry it at low temperature; (2) immersing the dried synthetic sponge in the carbon precursor solution, taking it out after it is completely soaked, and drying and curing it to obtain a foamed carbon precursor; (3) placing the carbon foam precursor into a high-temperature furnace for heating and carbonization to obtain high-porosity carbon foam.
2. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features Step 1 uses synthetic sponges such as polyurethane sponges and polyvinyl alcohol sponges.
3. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features In step 1, the porosity of the synthetic sponge used is above 90%, and the pore size is between 10ppi and 100ppi.
4. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features Step 1: Clean with deionized water, anhydrous ethanol or isopropanol; the drying temperature is not higher than 100°C.
5. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features The mass concentration of the organic resin in the carbon precursor solution in step 2 is 15% to 50%.
6. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features The carbon precursor solution in step 2 is a solution of an organic resin; the resin is one or any combination of phenolic resin, furfural resin, and benzoxazine; the solvent is ethanol, acetone or deionized water.
7. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features Step 2: drying and curing temperature 80-200°C, curing time 5-20h.
8. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features The synthetic sponge is a polyurethane sponge; the carbon precursor solution is a benzoxazine resin solution, and the mass concentration of the resin is 20-40%.
9. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features Step 3 The carbonization process is carried out in two stages; the first stage is to keep the temperature at 100-200°C, 400-550°C, and 700-1200°C for 1-5 hours at a heating rate of 0.5-5°C / min; the second stage is to keep the temperature at 2000-2300°C for 1-10 hours at a heating rate of 5-10°C / min.
10. The method for preparing high-porosity foamed carbon for silicon carbide crystal growth according to claim 1, Features Step 3: The carbonization process is carried out in an Ar gas atmosphere, the pressure in the high-temperature furnace is 10-80 kPa, and the Ar gas flow rate is 5-20 SLM.
Citation Information
Patent Citations
Mesh glassy carbon and preparation method thereof
CN116495720A
A silicon carbide crystal growth device for porous graphite embedding
CN218812232U
Production of carbon material coated with carbon coating film
JP1992164860A
A composite material of metal foam-carbon nanotube, the preparation method thereof and the use thereof
US20180123137A1