Porous carbon material and preparation method thereof, silicon carbon material, secondary battery and electronic equipment

By regulating the ultra-micropore and micropore ratio and crosslinking structure of porous carbon materials, the structural damage caused by volume changes during charging and discharging of silicon carbon materials is solved, and the cycle stability and rate performance of secondary batteries are improved, thus achieving the realization of the Higher energy density and conductivity.

CN118929651APending Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202411001979.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The volume expansion and contraction of silicon carbon materials during charging and discharging leads to structural damage, resulting in a decrease in the circulation performance of the secondary battery and side reactions with the electrolyte, affecting the battery performance.

Method used

By controlling the ratio of ultra-micropores and micropores of porous carbon materials, the internal density and compression strength are improved, the expansion rate of silicon carbon materials is slowed down, and the conductive network is formed through cross-linked structures to improve the anti-expansion, circulation and Rate performance.

Benefits of technology

It significantly improves the cycle stability and energy density of secondary batteries, reduces the breakage of silicon-carbon materials, enhances the conductivity and deintercalation ability of active substances, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929651A_ABST
    Figure CN118929651A_ABST
Patent Text Reader

Abstract

The invention provides a porous carbon material and a preparation method thereof, a silicon carbon material, a secondary battery and electronic equipment, and belongs to the technical field of energy storage. According to the porous carbon material, based on the pore volume of the porous carbon material, the volume ratio of ultra-micropores with the pore diameter smaller than or equal to 0.7 nm is P < 0 >%, the volume ratio of micropores with the pore diameter smaller than or equal to 2 nm is P < 1 >%, P < 0 > is larger than or equal to 2 and smaller than or equal to 28, and P < 1 > is larger than or equal to 92 and smaller than or equal to 100. The internal density of the porous carbon material is improved by controlling the micropore proportion of the porous carbon material, the structural stability and compression strength of the porous carbon material are improved, the expansion rate of the silicon-carbon material in the circulation process can be reduced, meanwhile, the surface area of the porous carbon material is increased, and deintercalation of active substances is promoted; and the expansion inhibition performance, the cycle performance and the rate capability of the secondary battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of energy storage technology, and specifically relates to a porous carbon material and a preparation method thereof, a silicon-carbon material, a secondary battery and an electronic device. Background Art

[0002] Silicon-carbon materials include silicon and carbon elements, and have the advantages of high capacity and stability. They have shown great potential as negative electrode materials for secondary batteries, especially in secondary batteries such as lithium-ion batteries and sodium-ion batteries.

[0003] However, silicon undergoes significant volume expansion and contraction during the charge and discharge process, which can easily lead to structural damage to the silicon-carbon material, resulting in problems such as surface peeling and particle pulverization. This causes the silicon-carbon material to easily react with the electrolyte during the charge and discharge cycle of the secondary battery, thereby causing the loss of active substances, further exacerbating the decay of the cycle performance and causing the performance of the secondary battery to decline. Therefore, how to optimize the structure of the silicon-carbon material and improve the cycle stability of the secondary battery has become an urgent problem to be solved in this field. Summary of the invention

[0004] In order to solve the above problems, the present application provides a porous carbon material and a preparation method thereof, a silicon-carbon material, a secondary battery and an electronic device. By controlling the micropore ratio of the porous carbon material to increase its internal density, the structural stability and compression strength of the porous carbon material are increased, and the expansion rate of the silicon-carbon material during the cycle process can be slowed down. At the same time, it is also beneficial to increase the surface area of ​​the porous carbon material, promote the deintercalation of active substances, and improve the expansion inhibition performance, cycle performance and rate performance of the secondary battery.

[0005] In a first aspect, the present application provides a porous carbon material, wherein based on the pore volume of the porous carbon material, the volume proportion of ultramicropores with a pore diameter less than or equal to 0.7 nm is P 0 %, the volume proportion of micropores with a pore size less than or equal to 2nm is P 1 %,2≤P 0 ≤28,92≤P 1 ≤100. The present application controls the volume ratio of ultramicropores and micropores in the porous carbon material, thereby providing space for silicon deposition while promoting uniform deposition of silicon, and making the porous carbon material have a high-density cross-linked structure inside, which can increase the stability and compression strength of the material structure, provide stable support for the silicon material, and thus better buffer the volume change and stress of silicon during the charging and discharging process, reduce the structural damage of the silicon material caused by volume expansion or contraction during the charging and discharging process, and improve the anti-expansion performance and cycle performance of the secondary battery. In addition, the above-mentioned microporous structure is also beneficial to increase the surface area of ​​the porous carbon material, promote the deintercalation of the active substance, and cooperate with the conductive network formed by the cross-linked structure to improve the rate performance of the secondary battery.

[0006] In some more preferred embodiments, 6.5≤P 0 ≤19.5,95≤P 1 ≤100. The volume ratio of ultramicropores and micropores in porous carbon materials is regulated to meet this condition. A higher micropore ratio can further improve the deposition uniformity of silicon and the structural stability of porous carbon materials, improve the expansion suppression performance and cycle performance of secondary batteries, and significantly improve the rate performance of secondary batteries by matching the volume ratio of ultramicropores.

[0007] In some embodiments, the specific surface area of ​​the porous carbon material is SA m 2 / g, 1059≤SA≤2486; and / or, the pore volume of the porous carbon material is Pv cm 3 / g, 0.52≤Pv≤1.6. The present application regulates the specific surface area and pore volume of the porous carbon material to meet the above ranges, so that it has a larger specific surface area and a rich microporous pore structure, which is beneficial to improving the adsorption capacity of silane gas and achieving a higher silicon deposition amount. It can also improve the mechanical strength and structural stability of the porous carbon material, and obtain a silicon-carbon material with high energy density and stable structure, so that the secondary battery has a higher energy density, while taking into account excellent rate performance, anti-expansion performance and cycle performance.

[0008] In some embodiments, the compressive strength of the porous carbon material is CS MPa, 161≤CS≤1968; preferably, 1096≤CS≤1878. The porous carbon material with high compressive strength provided in the present application can be used as a matrix to prepare a silicon-carbon negative electrode material with high compressive strength. By improving the strength of the porous carbon matrix, the strength of the silicon-carbon material can be improved, and the crushing of silicon-carbon particles caused by the rolling process of the pole piece preparation can be reduced, which is conducive to maintaining a high first coulomb efficiency and energy density, and can also improve the expansion inhibition performance and cycle performance of the secondary battery.

[0009] In some embodiments, the porous carbon material satisfies at least one of the following conditions: (1) the average ellipticity of the porous carbon material is ERm, 0.91≤ERm≤1; (2) the particle size Dv50 of the porous carbon material is Dμm, 5.2≤D≤9.8; (3) the compaction density of the porous carbon material at a pressure of 5000kgf is ρg / cm 3 , 0.45≤ρ≤0.7; (4) in the Raman spectrum of the porous carbon material, 0.8≤ID / IG≤1.5. By regulating the porous carbon material to meet at least one of the above conditions, combined with the above-mentioned ultra-micropore and micropore structures, the rate performance, expansion suppression performance and cycle performance of the secondary battery can be further improved.

[0010] In a second aspect, the present application provides a method for preparing any of the above-mentioned porous carbon materials, comprising the following steps: step 1, subjecting a phenolic compound, an acidic catalyst, a stabilizer and an aldehyde compound to a gradient heat preservation treatment under an inert atmosphere to obtain an organic precursor; the gradient heat preservation treatment comprises ... at a first temperature T 1 ℃ for the first heat preservation treatment, the heat preservation time is t 1 h, then at a second temperature T 2 ℃ for the second heat preservation treatment, the heat preservation time is t 2 h; where 20≤T 1 ≤100; 0.5≤t 1 ≤6; 60≤T 2 ≤150; 0.5≤t 2 ≤16; the mass ratio of the phenolic compound, the acidic catalyst and the aldehyde compound is 1:(1-5):(2-5); step 2, sequentially curing and carbonizing the organic precursor to obtain a carbide; step 3, mixing the carbide with an activator and performing an activation treatment to obtain a porous carbon material; the activator includes potassium hydroxide and sodium carbonate, and the mass ratio of potassium hydroxide to sodium carbonate is 1:(0.1-0.3); the temperature of the activation treatment is T 5 ℃, time is t 5 h; 621≤T 5 ≤854; 0.5≤t 5 ≤6. The present application controls the ratio of raw materials and catalysts in combination with gradient heat preservation treatment, and controls the activation treatment conditions to meet the above range, which can improve the crosslinking degree of the organic precursor, increase the micropore volume ratio of the porous carbon material, and make the porous carbon have a high-density crosslinked structure inside, which is beneficial to improving the rate performance, anti-swelling performance and cycle performance of the secondary battery when used in the secondary battery.

[0011] In some embodiments, the preparation method satisfies at least one of the following conditions: (1) the phenolic compound includes at least one of phenol, resorcinol, phloroglucinol, and bisphenol A; (2) the acidic catalyst includes at least one of hydrochloric acid, sulfuric acid, nitric acid, and oxalic acid; (3) the aldehyde compound includes at least one of formaldehyde, paraformaldehyde, furfural, and acetaldehyde; (4) the stabilizer includes at least one of polyvinyl alcohol, polyethylene glycol, hydroxymethyl cellulose, carboxymethyl cellulose, and polyvinyl pyrrolidone; (5) the mass ratio of the phenolic compound to the stabilizer is 1:(0.01-2.8); (6) the temperature of the curing treatment is T 3 ℃, time is t 3 h; 40≤T 3 ≤120; 0.5≤t 3 ≤6; (7) The temperature of carbonization treatment is T 4 ℃, time is t 4 h; 500≤T4 ≤1000; 0.5≤t 4 ≤6; (8) The mass ratio of the carbide to the activator is w, 0.1≤w≤1. The present application can further optimize the microporous structure of the porous carbon material and improve the rate performance, anti-swelling performance and cycle performance of the secondary battery by regulating the preparation method to meet at least one of the above conditions.

[0012] In a third aspect, the present application provides a silicon-carbon material, including the porous carbon material provided in the first aspect or the porous carbon material obtained by the preparation method provided in the second aspect. By regulating the ultra-micropore and micropore pore structure of the porous carbon, the conductivity and structural stability of the carbon matrix in the silicon-carbon material can be improved, thereby reducing the resistance of the silicon-carbon material and the volume expansion during the charge and discharge process, and improving the rate performance, anti-expansion performance and cycle performance of the secondary battery.

[0013] In a fourth aspect, the present application provides a secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode collector and a negative electrode active material layer arranged on at least one surface of the negative electrode collector; the negative electrode active material layer comprises the silicon-carbon material provided in the third aspect.

[0014] In a fifth aspect, the present application provides an electronic device, comprising the secondary battery provided in the fourth aspect.

[0015] Based on the porous carbon material and its preparation method, silicon-carbon material, secondary battery and electronic device provided by the present application, the present application can improve the structural stability and adsorption capacity of silane gas of the porous carbon material by improving the ultra-micropore and micropore structure of the porous carbon material. The porous carbon skeleton with high compressive strength can provide stable support for the silicon material, reduce the stress generated by the volume expansion of the silicon material during the charging and discharging process, and thus reduce the breakage of the silicon-carbon material. In addition, the cross-linked structure of the porous carbon can form a conductive network, improve the electrical conductivity of the porous carbon, and enable the secondary battery to have a higher energy density, while also taking into account the improvement of the anti-expansion performance, cycle performance and rate performance of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The pore distribution diagram of the porous carbon material of Examples 1-4;

[0017] Figure 2 The adsorption-desorption isotherms of the porous carbon materials of Examples 1-4;

[0018] Figure 3 XRD diagram of the porous carbon material of Examples 1-4;

[0019] Figure 4 The SEM images of the surface morphology of the porous carbon materials of Examples 1-4;

[0020] Figure 5SEM images of the cross-sectional morphology of the porous carbon materials of Examples 1-4. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0022] Silicon-carbon materials are often used as lithium-ion negative electrode materials to improve the overall energy density of secondary batteries due to their high lithium storage capacity. Silicon-carbon materials are often prepared from porous carbon by silane vapor deposition. During the research on silicon-carbon materials, the inventors found that silicon-carbon materials are often broken due to rolling during the manufacturing process of the pole piece due to insufficient strength, exposing silicon and causing more interfacial side reactions with the electrolyte, thus affecting the long-term cycle performance of the secondary battery.

[0023] In view of this, the present application provides a porous carbon material in a first aspect. Based on the pore volume of the porous carbon material, the volume proportion of ultra-micropores with a pore diameter less than or equal to 0.7 nm is P 0 %, the volume proportion of micropores with a pore size less than or equal to 2nm is P 1 %,2≤P 0 ≤28,92≤P 1 ≤100. In some embodiments, P 0 is 2, 3, 5, 6, 7, 8, 9, 11, 12, 13, 15, 16, 18, 19, 21, 22, 23, 24, 26, 27, 28 or a value within a range consisting of any two of these values. In some embodiments, P 1 It is a value within the range of 92, 93, 94, 95, 96, 97, 98, 99, 100 or any two of these values. The present application controls the volume ratio of ultra-micropores and micropores of the porous carbon material to conform to the above range, wherein the micropores provide conditions for the diffusion of silane gas, which is beneficial to the uniform deposition of nano-silicon and reduces the volume expansion problem of large-sized silicon particles; the combination of ultra-micropores and micropores can form a high-density cross-linked network structure inside the porous carbon, which not only forms a conductive network inside the silicon-carbon material to improve the conductivity of the silicon-carbon material, but also increases the structural stability and compression strength of the porous carbon material, reduces the volume change and stress of silicon during the charge and discharge process, reduces the structural damage caused by volume expansion or contraction of the silicon material during the charge and discharge process, and improves the rate performance, expansion inhibition and cycle performance of the secondary battery. Preferably, 6.5≤P 0 ≤19.5,95≤P 1 ≤100. The porous carbon material meeting this condition can further improve the rate performance, expansion suppression performance and cycle performance of the secondary battery.

[0024] In some embodiments, the specific surface area of ​​the porous carbon material is SA m 2 / g, 1059≤SA≤2486; for example, SA is 1059, 1065, 1170, 1223, 1321, 1412, 1484, 1577, 1630, 1667, 1738, 1851, 1914, 1985, 2041, 2115, 2207, 2280, 2358, 2416, 2486 or a value within the range formed by any two of these values. The present application controls the specific surface area of ​​the porous carbon material to conform to the above range. A higher specific surface area is beneficial to increasing the adsorption amount of silane gas during the preparation of silicon-carbon materials. The above-mentioned microporous pore structure can promote the uniform deposition of nano-silicon, and can also make the porous carbon material have a suitable pore volume, thereby improving the compression strength of the porous carbon material and improving the expansion inhibition and cycle performance of the secondary battery. On the other hand, the high specific surface area is also conducive to promoting the embedding and deintercalation of active substances such as lithium ions in silicon-carbon materials, and combined with the cross-linked network conductive structure, it can further improve the rate performance of secondary batteries.

[0025] In some embodiments, the pore volume of the porous carbon material is Pv cm 3 / g, 0.52≤Pv≤1.6. Exemplarily, Pv is 0.52, 0.55, 0.60, 0.69, 0.75, 0.79, 0.81, 0.90, 0.94, 1.00, 1.09, 1.11, 1.16, 1.22, 1.31, 1.32, 1.38, 1.45, 1.53, 1.56, 1.6 or a value within the range formed by any two of these values. By regulating the pore volume of the porous carbon material within the above range, the porous carbon material can have both a high silicon loading and a compressive strength, and obtain a silicon-carbon material with high energy density and stable structure, so that the secondary battery has a high energy density, while taking into account excellent anti-expansion performance and cycle performance.

[0026] In some embodiments, the compressive strength of the porous carbon material is CS MPa, 161≤CS≤1968; preferably, 1096≤CS≤1878. Exemplarily, CS is 161, 219, 280, 366, 456, 549, 705, 774, 861, 955, 1096, 1120, 1268, 1381, 1458, 1558, 1604, 1752, 1878, 1940, 1968 or a value within the range formed by any two of these values. The present application regulates the compressive strength of the porous carbon material to meet the above range, and cooperates with the above-mentioned pores and other structural features to resist the subsequent volume expansion of the silicon-carbon material during lithium ion embedding, reduce the breakage of the silicon-carbon material caused by expansion, and the material breakage caused by rolling during the manufacturing process of the battery material pole piece, reduce or avoid the exposure of active silicon caused by the breakage of the silicon-carbon material and the side reaction with the electrolyte, which is beneficial to improve the cycle performance and expansion performance of the secondary battery.

[0027] In some embodiments, the average ellipticity of the porous carbon material is ERm, 0.91≤ERm≤1. For example, ERm is 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1 or a value within the range formed by any two of these values. When the average ellipticity of the porous carbon material is regulated to meet the above range, combined with the pore structure characteristics of the porous carbon material, the stress on the silicon-carbon material during the rolling process can be further reduced, which is beneficial to reduce the breakage of the silicon-carbon material and the subsequent side reactions with the electrolyte, thereby improving the cycle performance of the secondary battery.

[0028] In some embodiments, the particle size Dv50 of the porous carbon material is Dμm, 5.2≤D≤9.8, for example, D is 5.2, 5.3, 5.5, 5.7, 6.0, 6.2, 6.6, 6.9, 7.0, 7.3, 7.4, 7.7, 8.1, 8.3, 8.5, 8.8, 9.0, 9.1, 9.5, 9.7, 9.8 or a value within the range formed by any two of these values. The present application regulates the particle size Dv50 of the porous carbon material to meet the above range, so that the porous carbon material can take into account both high compression strength and suitable specific surface area, which is beneficial to reduce the side reactions of the silicon-carbon material and the electrolyte, and improve the expansion inhibition performance and cycle performance of the secondary battery.

[0029] In some embodiments, the particle size distribution of the porous carbon material further comprises: Dv10 ≥ 2 μm, Dv99 ≤ 30 μm.

[0030] In some embodiments, the compaction density of the porous carbon material at a pressure of 5000 kgf is ρg / cm 3, 0.45≤ρ≤0.7; for example, ρ is 0.45, 0.46, 0.47, 0.48, 0.49, 0.51, 0.52, 0.54, 0.55, 0.56, 0.58, 0.59, 0.60, 0.61, 0.62, 0.64, 0.65, 0.67, 0.68, 0.69, 0.7 or a value in the range formed by any two of these values. When the compaction density of the porous carbon material is regulated within the above range, the energy density of the silicon-carbon material can be increased by cooperating with its microporous pore structure, while taking into account the higher compression strength, which is beneficial to improving the expansion inhibition performance and cycle performance of the secondary battery.

[0031] In some embodiments, in the Raman spectrum of the porous carbon material, 0.8≤ID / IG≤1.5. Exemplarily, the value of ID / IG is 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5 or a value in the range composed of any two of these values. The present application regulates the value of ID / IG to meet the above range, which can increase the active sites for depositing silicon in the porous carbon material, reduce the proportion of defect sites, and is conducive to increasing the silicon loading and deposition uniformity, improving the structural stability of the silicon-carbon material, taking into account the higher conductivity, and improving the expansion inhibition performance, rate performance and cycle performance of the secondary battery.

[0032] In a second aspect, the present application provides a method for preparing any of the above-mentioned porous carbon materials, comprising the following steps: step 1, subjecting a phenolic compound, an acidic catalyst, a stabilizer and an aldehyde compound to a gradient heat preservation treatment under an inert atmosphere to obtain an organic precursor; the gradient heat preservation treatment comprises ... at a first temperature T 1 ℃ for the first heat preservation treatment, the heat preservation time is t 1 h, then at a second temperature T 2 ℃ for the second heat preservation treatment, the heat preservation time is t 2 h; where 20≤T 1 ≤100; 0.5≤t 1 ≤6; 60≤T 2 ≤150; 0.5≤t 2 ≤16; the mass ratio of the phenolic compound, the acidic catalyst and the aldehyde compound is 1:(1-5):(2-5); step 2, sequentially curing and carbonizing the organic precursor to obtain a carbide; step 3, mixing the carbide with an activator and performing an activation treatment to obtain a porous carbon material; the activator includes potassium hydroxide and sodium carbonate, and the mass ratio of potassium hydroxide to sodium carbonate is 1:(0.1-0.3); the temperature of the activation treatment is T 5 ℃, time is t 5 h; 621≤T 5 ≤854; 0.5≤t 5≤6. In the present application, phenolic compounds, aldehyde compounds, acidic catalysts and stabilizers are subjected to gradient heat preservation treatment together, which can improve the crosslinking degree and mechanical strength of the organic precursor, and cooperate with the conditions of subsequent activation treatment, using the different activities of potassium hydroxide and sodium carbonate to intercalate the two into the carbide skeleton to form microporous and ultra-microporous pore structures, so that the porous carbon has a high-density crosslinked structure inside, and it is also helpful to control the pore volume and specific surface area of ​​the porous carbon, so as to obtain a porous carbon material with high compressive strength.

[0033] The inventors found that porous carbon materials usually use biomass, petroleum coke or resin as precursors. There are many macropores inside the biomass itself, so the matrix strength is not high, and it is difficult to improve its own strength through modification. Petroleum coke itself is soft carbon, and the porous carbon material particles prepared from it are not high in compression strength. Due to the differences in the preparation process of resin materials with different matrices, the carbon skeleton strength derived is also significantly different. Due to the low strength of the carbon matrix skeleton, it is difficult to provide sufficient strength support for the silicon-carbon material particles. In the preparation of the negative electrode plate, in order to increase the volume energy density, the plate is rolled, and the silicon-carbon particles are broken due to rolling. The exposed silicon material will react with the electrolyte to continuously form an SEI film. As the cycle proceeds, the SEI continues to thicken and consume the silicon material and the electrolyte, resulting in the attenuation of the overall cycle life. This application forms ultra-micropores and micropore distribution structures in the porous carbon material by increasing the cross-linking degree of the organic precursor and cooperating with the activation treatment step, thereby improving the compression strength of the porous carbon material and thus improving the compression resistance of the silicon-carbon material itself. Porous carbon materials with a certain specific surface area and pore volume are prepared by carbonization and activation treatments. The pore volume and pore size distribution are adjusted and silicon material is appropriately deposited. The volume of the reserved pores provides space for lithium expansion of silicon to buffer the volume expansion of silicon, thereby giving full play to the excellent characteristics of high energy density of silicon materials, while improving the expansion suppression performance, cycle performance and rate performance of secondary batteries.

[0034] In some embodiments, during the gradient heat preservation treatment, 20≤T 1 ≤100; 0.5≤t 1 ≤6; for example, T 1 is 20, 21, 26, 32, 33, 39, 42, 46, 52, 58, 59, 66, 69, 73, 75, 81, 86, 91, 94, 96, 100 or a value in the range of any two of these values, t 1 It is 0.5, 0.9, 1.1, 1.6, 2.1, 2.4, 2.9, 3.4, 3.5, 4.1, 4.6, 5.0, 5.3, 5.7, 6 or a value within the range consisting of any two of these values.

[0035] In some embodiments, 60≤T 2≤150; 0.5≤t 2 ≤16; for example, T 2 is 60, 62, 68, 72, 75, 82, 87, 92, 98, 102, 105, 111, 115, 117, 122, 129, 134, 139, 145, 148, 150 or a value within the range of any two of these values, t 2 The value is 0.5, 0.8, 1.3, 2.2, 3.0, 4.4, 5.3, 5.6, 6.3, 7.5, 8.7, 9.3, 10.1, 10.8, 11.5, 12.7, 13.1, 13.7, 14.6, 15.6, 16 or a value within the range consisting of any two of these values.

[0036] In some embodiments, T 1 <T 2 Controlling the above-mentioned gradient heat preservation treatment conditions can improve the cross-linking degree of the organic precursor, which is beneficial to the subsequent formation of a suitable microporous pore structure.

[0037] In some embodiments, the mass ratio of the phenolic compound, the acidic catalyst and the aldehyde compound is 1:(1-5):(2-5). For example, when the mass fraction of the phenolic compound is 1 part, the mass fraction of the acidic catalyst is 1 part, 2 parts, 3 parts, 4 parts, 5 parts or a value in the range of any two thereof, and the mass fraction of the aldehyde compound is 2 parts, 3 parts, 4 parts, 5 parts or a value in the range of any two thereof.

[0038] In some embodiments, 621≤T 5 ≤854; 0.5≤t 5 ≤6. For example, T 5 is 621, 625, 642, 650, 658, 678, 688, 705, 716, 723, 738, 754, 763, 778, 784, 798, 817, 818, 839, 853, 854 or a value in the range consisting of any two of these values, t 5 The present invention is 0.5, 0.9, 1.1, 1.6, 2.1, 2.4, 2.9, 3.4, 3.5, 4.1, 4.6, 5.0, 5.3, 5.7, 6 or a value within the range formed by any two of these values. The present invention can promote the formation of sufficient pore structure of carbide by regulating the temperature and time of activation treatment, and is beneficial to improving the structural strength of the porous carbon precursor.

[0039] In some embodiments, the phenolic compound includes at least one of phenol, resorcinol, phloroglucinol, and bisphenol A.

[0040] In some embodiments, the acidic catalyst includes at least one of hydrochloric acid, sulfuric acid, nitric acid, and oxalic acid.

[0041] In some embodiments, the aldehyde compound includes at least one of formaldehyde, paraformaldehyde, furfural, and acetaldehyde.

[0042] In some embodiments, the stabilizer includes at least one of polyvinyl alcohol (PVA), polyethylene glycol (PEG), hydroxymethyl cellulose (HEC), carboxymethyl cellulose (CMC), and polyvinyl pyrrolidone (PVP).

[0043] In some embodiments, the weight ratio of the phenolic compound to the stabilizer is 1:(0.01-2.8). For example, when the weight fraction of the phenolic compound is 1 part, the weight fraction of the stabilizer is 0.01 part, 0.13 part, 0.17 part, 0.36 part, 0.50 part, 0.73 part, 0.79 part, 1.00 part, 1.07 part, 1.24 part, 1.47 part, 1.50 part, 1.63 part, 1.90 part, 2.05 part, 2.11 part, 2.36 part, 2.45 part, 2.53 part, 2.65 part, 2.8 part or a value in the range consisting of any two of them.

[0044] In some embodiments, the curing temperature is T 3 ℃, time is t 3 h; 40≤T 3 ≤120; 0.5≤t 3 ≤6. For example, T 3 is 40, 42, 46, 49, 54, 59, 62, 65, 70, 75, 78, 86, 88, 93, 98, 102, 105, 111, 113, 119, 120 or a value within the range of any two of these values, t 3 It is 0.5, 0.9, 1.1, 1.6, 2.1, 2.4, 2.9, 3.4, 3.5, 4.1, 4.6, 5.0, 5.3, 5.7, 6 or a value within the range consisting of any two of these values.

[0045] In some embodiments, the curing process includes mixing an organic precursor with a curing agent at a temperature of T 3 The curing treatment was carried out under the condition of ℃, and the treatment time was t 3 h. Optionally, the curing agent includes at least one of ammonia water, hexamethylenetetramine, melamine or triethylamine. Optionally, the mass concentration of the curing agent is 0.05% to 20%. These curing agents can participate in changing the molecular structure and properties of the organic precursor, improve the polymerization and curing degree of the organic precursor, and help improve the effect of subsequent carbonization treatment and activation treatment.

[0046] In some embodiments, the carbonization treatment is performed under an inert atmosphere, and the inert atmosphere is selected from at least one of nitrogen and argon.

[0047] In some embodiments, the temperature of the carbonization treatment is T 4 ℃, time is t 4 h; 500≤T 4 ≤1000; 0.5≤t 4 ≤6. For example, T 4 is 500, 540, 570, 600, 630, 660, 680, 700, 710, 740, 760, 790, 820, 850, 870, 900, 940, 950, 990, 1000 or a value in the range of any two of these values, t 4 The carbonization temperature and time can be adjusted to reduce the residual organic matter and form a denser pore structure, which is beneficial to the subsequent activation and helps to promote the formation of a spherical morphology of the carbon precursor.

[0048] In some embodiments, the mass ratio of the carbide to the activator is w, 0.1≤w≤1. For example, w is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, or a value in the range formed by any two of these values. The present application regulates the mass ratio of the carbide to the activator within the above range, which can improve the activation effect of the carbide, form a suitable microporous pore structure, and improve the compressive strength of the porous carbon material.

[0049] In some embodiments, after the activation treatment is completed and cooled to room temperature, the material is taken out and washed with deionized water multiple times and neutralized with a small amount of hydrochloric acid until the impurities are removed. The material is then dried at 120° C. for 12 hours to obtain a porous carbon material.

[0050] In a third aspect, the present application provides a silicon-carbon material, including the porous carbon material provided in the first aspect of the present application or the porous carbon material obtained by the preparation method provided in the second aspect. The silicon-carbon material of the present application utilizes the microporous pore structure of the porous carbon material to improve the compression strength. On the one hand, it can resist the pressure during the rolling process without breaking, thereby maintaining the integrity of the silicon-carbon material structure. On the other hand, it can restrain the volume expansion caused by the insertion of lithium ions, so that the secondary battery has excellent cycle and expansion performance when used in the secondary battery; in addition, the conductive network and high specific surface area of ​​the porous carbon are conducive to improving the rate performance of the secondary battery.

[0051] The present application has no special restrictions on the preparation method of silicon-carbon material, as long as it can meet the purpose of the present application. For example, the porous carbon material provided in the first aspect of the present application is used as a skeleton, and nano-scale silicon particles are deposited on the surface and / or in the pores of the porous carbon skeleton material through silane vapor deposition to prepare the silicon-carbon material.

[0052] In some embodiments, the silicon-carbon material includes a porous carbon material and a silicon material located on the surface and / or inside the pores of the porous carbon material. When the porous carbon material provided in the present application is used as a skeleton for silane vapor deposition, it can limit the growth of silicon grains through nanoscale pores and can limit the silicon grains within the nanoscale range, thereby avoiding the pulverization problem caused by the expansion of large-sized silicon particles embedded in lithium, and thus after being used in a secondary battery, the latter can have both high energy density, anti-expansion performance and cycle performance.

[0053] In a fourth aspect, the present application provides a secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode collector and a negative electrode active material layer arranged on at least one surface of the negative electrode collector; the negative electrode active material layer comprises the silicon-carbon material provided in the third aspect of the present application.

[0054] The secondary battery of the present application is not particularly limited, and may include, but is not limited to, a lithium-ion secondary battery (also called a lithium-ion battery) or a sodium-ion secondary battery.

[0055] In the present application, the above-mentioned "negative electrode active material layer disposed on at least one surface of the negative electrode current collector" means that the negative electrode active material layer can be disposed on the surface on one side in the thickness direction of the negative electrode current collector, or on the surfaces on both sides in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector, or it can be a partial area of ​​the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the thickness of the negative electrode active material layer, as long as the purpose of this application can be achieved. For example, the thickness of the single-sided negative electrode active material layer can be 30μm to 160μm.

[0056] In some embodiments, the negative electrode active material layer further includes natural graphite and / or artificial graphite.

[0057] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, composite current collector (such as carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector), polymer substrate coated with conductive metal or any combination thereof. The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 10μm.

[0058] In the present application, the negative electrode active material layer may also include a negative electrode binder, which may include but is not limited to polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyacrylic acid (PAA), styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin or at least one of nylon.

[0059] In the present application, the negative electrode active material layer may also include a conductive agent. The present application has no particular restrictions on the type of conductive agent in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to carbon-based materials, metal-based materials, conductive polymers and mixtures thereof. In some embodiments, the carbon-based material is selected from carbon black, acetylene black, Ketjen black, carbon fiber or any combination thereof. In some embodiments, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum or silver. In some embodiments, the conductive polymer is a polyphenylene derivative. The present application has no particular restrictions on the mass ratio of the negative electrode material, the conductive agent and the negative electrode binder in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the loading amount of the negative electrode active material in the negative electrode sheet is 1.0 mg / cm 2 Up to 1.5 mg / cm 2 .

[0060] In the present application, there is no special restriction on the positive electrode, as long as the purpose of the present application can be achieved. For example, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector. The above-mentioned "positive electrode active material layer located on at least one surface of the positive electrode current collector" means that the positive electrode active material layer can be located on one surface of the positive electrode current collector along its own thickness direction, or on two surfaces of the positive electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of ​​the surface of the positive electrode current collector, or it can be a partial area of ​​the surface of the positive electrode current collector. There is no special restriction in the present application, as long as the purpose of the present application can be achieved.

[0061] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate.

[0062] The positive electrode active material layer of the present application includes a positive electrode active material. The present application has no particular limitation on the type of the positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include lithium nickel cobalt manganese oxide (LiNi 0.90 Co 0.05 Mn 0.05 O 2 (NCM955), NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO 2 ), at least one of lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganate, spinel lithium nickel manganate and lithium titanate. In the present application, the positive electrode active material may also contain non-metallic elements, for example, the non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur. In the present application, there is no particular restriction on the thickness of the positive current collector and the positive active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive current collector is 5μm to 20μm, and the thickness of the single-sided positive active material layer is 30μm to 120μm.

[0063] In the present application, the positive electrode active material layer may further include a positive electrode binder and a conductive agent. The present application does not particularly limit the type of positive electrode binder in the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the positive electrode binder may include but is not limited to polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified styrene butadiene rubber (SBR) or polyurethane. In some embodiments, the polyolefin binder includes at least one of polyethylene, polypropylene, polyolefin ester, polyolefin alcohol or polyacrylic acid.

[0064] The present application has no particular restrictions on the type of conductive agent in the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent can be the same type as the conductive agent in the above-mentioned negative electrode active material layer. In some embodiments, the conductive agent includes carbon-based materials, such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black or carbon fiber; metal-based materials, such as metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof. The present application has no particular restrictions on the mass ratio of the positive electrode active material, the conductive agent, and the positive electrode binder in the positive electrode active material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, the loading amount of the positive electrode active material in the positive electrode sheet is 4.0 mg / cm 2 Up to 10.0mg / cm 2 .

[0065] In the present application, the secondary battery also includes an electrolyte. According to some embodiments of the present application, the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include, but is not limited to: lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2 ), Lithium Bis(trifluoromethanesulfonyl)imide {LiN(CF 3 SO 2 ) 2 , LiTFSI)}, Li(N(SO 2 F) 2 ), LiFSI}, lithium bis(oxalatoborate){LiB(C 2 O 4 ) 2 , LiBOB}, Lithium difluorooxalatoborate {LiBF 2 (C 2 O 4 )、LiDFOB}、LiNO 3 、LiClO 4 、LiB(C 6 H 5 ) 4 、LiCH 3 SO 3 、LiCF 3 SO 3 、LiC(SO 2 CF 3 ) 3 , Li 2 SiF 6, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or lithium difluoroborate. The present application does not limit the content of lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. The present application has no special restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved. For example, the non-aqueous solvent may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds, cyclic carbonate compounds or fluorocarbonate compounds. The above-mentioned chain carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or ethyl methyl carbonate (EMC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate or vinyl ethylene carbonate. The fluorinated carbonate compound may include, but is not limited to, at least one of fluorinated ethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The above-mentioned ether compound may include, but is not limited to, at least one of 1,3-dioxolane (DOL), ethylene glycol dimethyl ether (1,2-dimethoxyethane, DME), dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include, but are not limited to, at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0066] The secondary battery of the present application also includes a separator. The material and shape of the separator used in the secondary battery of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application.

[0067] For example, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be selected.

[0068] A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polyvinylidene fluoride and poly (vinylidene fluoride-hexafluoropropylene).

[0069] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.

[0070] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and the present application has no special restrictions. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.

[0071] In a fifth aspect, the present application provides an electronic device, comprising the secondary battery provided in the fourth aspect of the present application.

[0072] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0073] The following uses lithium-ion batteries as an example to illustrate the solution of the present application in combination with the following specific embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all from common commercial products, and the devices or equipment used are all purchased from conventional market sales channels.

[0074] Test Method

[0075] Specific surface area, pore volume and pore size test:

[0076] The porous carbon material was tested using a physical adsorption instrument (model: ipore 620). The process included: taking 0.15 g of porous carbon material as a sample and placing it in a sample tube, first degassing it at 200°C for 6 hours, and then testing the adsorption amount of argon by the sample at different relative pressures to draw the isothermal adsorption curve of the sample, and then using BET fitting to calculate the specific surface area of ​​the sample, calculate the single-point adsorption pore volume of the sample, and use NLDFT to calculate the pore size distribution, and then calculate the volume ratio of ultramicropores and micropores based on the pore volume.

[0077] Compression strength test:

[0078] The test was conducted using a micro-particle compression tester (model: MCT-210). 0.05 g of the porous carbon material to be tested was uniformly dispersed by ultrasonication in 10 ml of ethanol. The dispersion was placed on the test platform. After the dispersion dried, a single particle of the porous carbon material to be tested was randomly selected as a test particle sample. The compression strength of the test particle sample was tested. The compression strength = 2.48 × P / (3.14 × d × d), where d is the diameter of the test particle sample, and P is the pressure value when the test particle sample breaks. A total of 10 test particle samples were selected, and the compression strength of the 10 test particle samples was arithmetic averaged to obtain the compression strength of the porous carbon material to be tested.

[0079] Average ellipticity test:

[0080] The particle sphericity analyzer (model: Occhio 500nanoXY) was used for testing. 0.5 g of the porous carbon material sample was ultrasonically dispersed in 10 ml of ethanol. The dispersion was added into the instrument for sample sphericity analysis to obtain the average ellipticity of the porous carbon material sample.

[0081] Particle size test:

[0082] The particle size of the porous carbon material was tested using a Malvern particle size tester (model: Mastersizer 3000). The porous carbon material sample was dispersed in water. After ultrasonic treatment for 30 minutes, the dispersion sample was added to the Malvern particle size tester to test the particle size distribution of the porous carbon material and obtain the Dv10, Dv50 and Dv99 of the porous carbon sample to be tested.

[0083] Compaction density test:

[0084] The compaction density of the porous carbon material was tested using a powder compaction density tester (model: UTM 7305). The porous carbon material sample was added to a compaction mold, and the compaction mold was placed on the powder compaction density measuring instrument. The compaction density of the porous carbon material sample was tested under a pressure of 5000 kgf.

[0085] ID / IG test:

[0086] The graphitization degree (ID / IG) of porous carbon materials was analyzed by Raman spectrometer (model: HR Evolution). The porous carbon material sample was placed in the sample tank, and the surface was flattened with a glass slide. The Raman spectrometer was used to collect the graphitization degree (ID / IG) of the porous carbon material sample at 150 cm -1 Up to 3500cm -1 The ID / IG values ​​of the porous carbon material samples were then analyzed.

[0087] Surface morphology test of porous carbon materials:

[0088] The surface morphology of the porous carbon sample was analyzed using a scanning electron microscope (model: sigma-02-33). The porous carbon sample to be tested was dispersed on a conductive adhesive, and then the surface morphology was observed under different magnifications (500-30000X) using a scanning electron microscope.

[0089] Porous carbon material cross-sectional morphology test:

[0090] A scanning electron microscope (model: sigma-02-33) was used to analyze the cross-sectional morphology characteristics of the porous carbon material sample. The porous carbon material and the binder were mixed evenly and coated on a copper foil to obtain a sample to be tested. The sample to be tested was then subjected to argon ion cross-sectional polishing to obtain a CP sample. The cross-sectional morphology characteristics of the CP sample were then observed under a scanning electron microscope.

[0091] XRD test:

[0092] The test was carried out using an XRD powder diffractometer (model: BRUKER D8 Advance): a porous carbon material was taken as the sample to be tested, the sample to be tested was first sieved with a 200-mesh sieve, then the powder under the sieve was put into the sample pool, and then the surface was flattened, and the excess powder around was cleaned up, and the prepared sample to be tested was placed in the XRD powder diffractometer, the sample to be tested was tested, and the XRD spectrum was collected.

[0093] Rate performance test:

[0094] Take the lithium ion battery of the embodiment / comparative example to be tested and place it at a test temperature of 25°C for 5 minutes, then charge the lithium ion battery to 4.45V at a constant current of 0.7C, and then charge it to 0.05C at a constant voltage of 4.45V; let it stand for 5 minutes, then discharge it to 3.0V at a constant current of 0.2C, and record the 0.2C discharge capacity; then let it stand for 5 minutes, repeat the above charging process, and then discharge it at a constant current of 2C, and record the 2C discharge capacity. Rate capacity retention rate = 2C discharge capacity / 0.2C discharge capacity × 100%.

[0095] Cycle performance test:

[0096] At a test temperature of 25°C, let the lithium-ion battery to be tested stand for 5 minutes, and record the initial thickness MMC0 of the lithium-ion battery. Perform 3.4C step charging on the lithium-ion battery. The 3.4C step charging includes: charging the lithium-ion battery to 4.25V with a current of 3.4C, then charging to 4.4V with a constant current of 2C, then charging to 4.50V with a constant current of 1C, and then charging to 0.05C with a constant voltage of 4.50V. Then let it stand for 5 minutes, and then discharge to 3.0V with a constant current of 0.5C, let it stand for 5 minutes, and record the discharge capacity C1 of the lithium-ion battery. After the above 3.4C step charging / 0.5C discharge charge and discharge cycle process is cycled 400 times, record the thickness MMC1 and discharge capacity C2 of the lithium-ion battery.

[0097] Cycle capacity retention rate (%) = C2 / C1×100%.

[0098] Cycle thickness expansion ratio (%) = (MMC1-MMC0) / MMC0×100%.

[0099] Example 1-1

[0100] Preparation of porous carbon materials

[0101] The method for preparing the porous carbon material of this embodiment comprises the following steps:

[0102] Step 1: Add phenol (phenol compound), hydrochloric acid (acid catalyst), and polyvinyl alcohol (stabilizer) into a three-necked flask at a mass ratio of 1:2:1.7, mix well, add an aqueous solution of formaldehyde (aldehyde compound), control the mass ratio of phenol to formaldehyde to be 1:2, and perform gradient heat preservation treatment under an inert atmosphere. The gradient heat preservation treatment includes heating at 100°C (first temperature T 1 ℃) for 2h(t 1 h), then at 150°C (second temperature T 2 ℃) for the second heat preservation treatment, the heat preservation time is 2h (t 2 h), and then filtered and washed with clean water to obtain an organic precursor.

[0103] Step 2: Mix the organic precursor with 2% ammonia water (curing agent) and then heat at 60°C (T 3 ℃) for 2h(t 3 h), after the curing treatment is completed, the solidified product is allowed to stand for 1 hour, and then filtered, washed and dried to obtain a solidified product. The solidified product is heated to 750°C (T 4 ℃), and then carbonized at this temperature for 2h (t 4 h), and cooling to room temperature after the reaction is completed to obtain a carbide.

[0104] Step 3: Carbide and an activator are mixed in a mass ratio of 1:2 (w=0.5) and then activated to obtain a porous carbon material; the activator includes potassium hydroxide and sodium carbonate, and the mass ratio of potassium hydroxide to sodium carbonate is 1:0.2; the temperature of the activation treatment is 700°C (T 5 ℃), time is 1h(t 5 h). After the activation treatment is completed and cooled to room temperature, the material is taken out and washed with deionized water for multiple times and neutralized with a small amount of hydrochloric acid until the impurities are removed. The material is then dried at 120° C. for 12 hours to obtain a porous carbon material.

[0105] The compaction density of the porous carbon material in this embodiment at a pressure of 5000 kgf is 0.53 g / cm 3 ; In the Raman spectrum of the porous carbon material of this embodiment, ID / IG=1.1.

[0106] Preparation of silicon-carbon materials

[0107] The prepared porous carbon material is placed in a fluidized bed deposition equipment, nitrogen is introduced to fluidize the porous carbon, and then the temperature is increased by 5°C per minute to a preset temperature of 500°C, and silane gas is introduced to react for 7.5 hours; thereafter, the temperature is increased to 600°C, and acetylene gas is introduced to form a carbon coating layer on the silicon-carbon surface. After the reaction is completed, the temperature is cooled to room temperature to obtain a silicon-carbon material.

[0108] Preparation of negative electrode

[0109] Graphite, silicon-carbon material prepared according to the embodiment and comparative example, conductive agent (carbon black) and binder PAA were mixed in a weight ratio of 70:15:5:10, and a proper amount of water was added, and kneaded at a solid content of 65wt%; and then a proper amount of water was added to adjust the viscosity of the slurry to 5000Pa·s to prepare a negative electrode slurry. The prepared negative electrode slurry was coated on a negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode.

[0110] Preparation of positive electrode

[0111] LiCoO 2 The positive electrode slurry is prepared by fully stirring and mixing carbon black and polyvinylidene fluoride (PVDF) in a N-methylpyrrolidone solvent system at a weight ratio of 95:2.5:2.5. The positive electrode slurry is coated on a positive electrode current collector aluminum foil, dried, and cold pressed to obtain a positive electrode.

[0112] Preparation of electrolyte

[0113] In a dry argon environment, LiPF was added to a solvent of propylene carbonate, ethylene carbonate, propyl propionate, and ethyl propionate (weight ratio of 2:1:1:2). 6 and fluoroethylene carbonate are uniformly mixed to obtain an electrolyte, wherein, based on the mass of the electrolyte, LiPF 6 The mass percentage of is 12.5%, and the mass percentage of fluoroethylene carbonate is 3.5%.

[0114] Preparation of diaphragm

[0115] A polyethylene / polypropylene composite porous polymer film with a thickness of 7 μm was used as the isolation membrane.

[0116] Preparation of lithium-ion batteries

[0117] Stack the positive electrode, separator and negative electrode in order, so that the separator is between the positive electrode and the negative electrode to play an isolating role. Wind to obtain a bare cell. Place the bare cell in an outer package, inject electrolyte and package. After the formation, degassing, trimming and other process flows, a lithium-ion battery is obtained.

[0118] The porous carbon materials of the embodiments and comparative examples in Table 1 are different from those of Example 1-1 only in that the preparation method of the porous carbon materials is adjusted according to the parameters in Table 1. Wherein N1 is potassium hydroxide, N2 is sodium carbonate, and the ratios involved are all mass ratios.

[0119] Table 1

[0120]

[0121]

[0122] The porous carbon materials of the embodiments and comparative examples in Table 2 are different from those of Example 1-1 only in that the preparation method of the porous carbon materials is adjusted according to the parameters in Table 2.

[0123] Table 2

[0124] serial number Phenol: Stabilizer <![CDATA[T 3 (℃)]]> <![CDATA[t 3 (h)]]> <![CDATA[T 4 (℃)]]> <![CDATA[T 4 (h)]]> Example 2-1 1:2.8 60 2 750 2 Example 2-2 1:0.1 60 2 750 2 Example 2-3 1:1.3 60 2 750 2 Embodiment 2-4 1:1.3 50 3 750 2 Embodiment 2-5 1:1.3 90 1 750 2 Embodiment 2-6 1:3 60 2 750 2 Embodiment 2-7 1:0.8 60 2 1000 2 Embodiment 2-8 1:0.8 60 2 500 2 Embodiment 2-9 1:0.8 60 2 450 2

[0125] The porous carbon materials of the embodiments and comparative examples were tested according to the above test method. The test results are shown in Table 3.

[0126] Table 3

[0127]

[0128]

[0129] As can be seen from Table 3, the volume proportion of ultra-micropores with a pore size less than or equal to 0.7 nm in the porous carbon material controlled by the present application is P 0 %, the volume proportion of micropores with a pore size less than or equal to 2nm is P 1 %,2≤P 0 ≤28,92≤P 1 ≤100, the porous carbon material has a high-density cross-linked structure inside, which can improve the rate performance, inhibit expansion performance and cycle performance of lithium-ion batteries. In particular, when 6.5≤P 0 ≤19.5, and 95≤P 1 When ≤100, it is beneficial to improve the compressive strength and structural stability of the porous carbon material, and the rate performance, expansion inhibition performance and cycle performance of the lithium-ion battery are further improved.

[0130] In particular, based on the above-mentioned microporous pore structure, the specific surface area of ​​the porous carbon material is adjusted to SAm 2 / g, 1059≤SA≤2486, and / or adjusting the pore volume of the porous carbon material to Pv cm 3 / g, 0.52≤Pv≤1.6, and the crystallite size g nm satisfies 0.88≤g≤4.20, which can give it a large specific surface area and rich microporous pore structure, further improving the rate performance, expansion inhibition performance and cycle performance of lithium-ion batteries.

[0131] In particular, the present application further regulates the compressive strength CS MPa of the porous carbon material to satisfy 161≤CS≤1968, preferably 1096≤CS≤1878, which, when combined with the above-mentioned microporous pore structure, enables the lithium-ion battery to have excellent rate performance, expansion suppression performance and cycle performance.

[0132] In particular, by regulating the average ellipticity of the porous carbon material to ERm, 0.91≤ERm≤1, and regulating the particle size Dv50 of the porous carbon material to Dμm, 5.2≤D≤9.8, it can have a suitable specific surface area and pore volume, so that the lithium-ion battery can exhibit more significant rate performance, expansion inhibition performance and cycle performance.

[0133] In addition, in combination with the data of Tables 1 to 3, it can be seen that the application controls the activator to include potassium hydroxide and sodium carbonate, and the mass ratio of potassium hydroxide and sodium carbonate is 1: (0.1-0.3), and the activation treatment conditions are adjusted to meet the above range, which can improve the crosslinking degree of the organic precursor and increase the micropore volume proportion of the porous carbon material. Among them, as the amount of activator increases, the pore volume of the porous carbon material continues to increase, and the specific surface area first increases and then decreases. The reason may be that the proportion of mesopores with a pore size exceeding 2nm increases, which contributes more pore volume and reduces the specific surface area. On the other hand, as the activation temperature increases, the pore volume tends to increase, while the specific surface area decreases, which may be due to the deepening of the degree of activation, more carbon is etched away, forming more macropores, thereby reducing the specific surface area.

[0134] On this basis, the mass ratio of phenolic compounds, acidic catalysts and aldehyde compounds is further controlled to be 1: (1-5): (2-5), and the gradient heat preservation treatment conditions are matched, so that the porous carbon can have a high-density cross-linked structure inside, improve the specific surface area and pore volume of the porous carbon material, and improve the compressive strength of the porous carbon material, which is beneficial to the application in lithium-ion batteries. When the catalyst concentration is increased, the particle size Dv50 of the porous carbon material has an increasing trend, and the compressive strength increases. It is due to the increase in the catalyst concentration, which accelerates the polymerization and cross-linking reactions, thereby increasing the resin ball diameter of the organic precursor, and the internal cross-linking degree is improved, and the stable and powerful cross-linked network formed internally is formed, thereby increasing the strength of the carbon skeleton. In particular, the mass ratio of the carbide and the activator is w, 0.1≤w≤1, which can further improve the microporous pore structure of the porous carbon material and improve the above-mentioned performance of the lithium-ion battery.

[0135] In particular, the present application regulates the mass ratio of phenolic compounds and stabilizers to 1: (0.01-2.8), and as the concentration of the stabilizer increases, the spherical diameter of the porous carbon tends to decrease, so that under the same activation conditions, the smaller the diameter of the carbon, the larger the specific surface area and pore volume after activation, and correspondingly due to the increase in pore volume, the compressive strength of the porous carbon material tends to decrease. And the curing treatment and carbonization treatment meet the above conditions, which can further optimize the microporous pore structure of the porous carbon material, and make the porous carbon material have a suitable particle size distribution, improve the specific surface area and pore volume of the porous carbon graphite material, and make the lithium-ion battery show more excellent rate performance, anti-expansion performance and cycle performance.

[0136] Figure 1 is a pore distribution diagram of the porous carbon material of Examples 1-4, wherein the pore volume proportion P of micropores with a pore diameter less than or equal to 2 nm 1 % is 100%, the pore volume proportion of ultra-micropores with a pore size less than or equal to 0.7nm is P 0 % is 20%.

[0137] Figure 2 It is the adsorption-desorption isotherm diagram of the porous carbon material of Examples 1-4. From the adsorption and desorption isotherm data, it can be seen that the adsorption and desorption isotherms are almost completely overlapped, and the difference between the adsorption volume and the desorption volume is very small, which is a typical microporous material.

[0138] Figure 3 1 is the XRD diagram of the porous carbon material of Example 1-4. It can be seen from the XRD diagram that the porous carbon material of this example exhibits typical amorphous carbon characteristics.

[0139] Figure 4 The SEM images of the surface morphology of the porous carbon material of Examples 1-4 show that the porous carbon material of this example has a material morphology similar to a perfect sphere and has a relatively high average ellipticity.

[0140] Figure 5 The SEM images of the cross-sectional morphology of the porous carbon material of Examples 1-4 show that the porous carbon material of this example has a relatively dense structure inside, which is beneficial to the improvement of the compressive strength.

[0141] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the principles of the present application should be included in the protection scope of the present application.

Claims

1. A porous carbon material, It is characterized in that Based on the pore volume of the porous carbon material, the volume proportion of ultramicropores with a pore size less than or equal to 0.7 nm is P 0 %, the volume proportion of micropores with a pore size less than or equal to 2nm is P 1 %,2≤P 0 ≤28,92≤P 1 ≤100.

2. The porous carbon material according to claim 1, It is characterized in that 6.5≤P 0 ≤19.5,95≤P 1 ≤100。 3. The porous carbon material according to claim 1 or 2, It is characterized in that The specific surface area of ​​the porous carbon material is SAm 2 / g, 1059≤SA≤2486; and / or, The pore volume of the porous carbon material is Pv cm 3 / g, 0.52≤Pv≤1.

6.

4. The porous carbon material according to claim 1 or 2, It is characterized in that The compressive strength of the porous carbon material is CS MPa, 161≤CS≤1968; preferably, 1096≤CS≤1878.

5. The porous carbon material according to claim 1 or 2, It is characterized in that The porous carbon material satisfies at least one of the following conditions: (1) The average ellipticity of the porous carbon material is ERm, 0.91≤ERm≤1; (2) The particle size Dv50 of the porous carbon material is D μm, 5.2≤D≤9.8; (3) The compaction density of the porous carbon material under a pressure of 5000 kgf is ρg / cm 3 , 0.45≤ρ≤0.7; (4) In the Raman spectrum of the porous carbon material, 0.8≤ID / IG≤1.

5.

6. A method for preparing a porous carbon material according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Step 1, subjecting a phenolic compound, an acidic catalyst, a stabilizer and an aldehyde compound to a gradient heat preservation treatment under an inert atmosphere to obtain an organic precursor; The gradient heat preservation treatment includes a first temperature T 1 ℃ for the first heat preservation treatment, the heat preservation time is t 1 h, then at a second temperature T 2 ℃ for the second heat preservation treatment, the heat preservation time is t 2 h; where 20≤T 1 ≤100; 0.5≤t 1 ≤6; 60≤T 2 ≤150; 0.5≤t 2 ≤16; The mass ratio of the phenolic compound, the acidic catalyst and the aldehyde compound is 1:(1-5):(2-5); Step 2, subjecting the organic precursor to a curing treatment and a carbonization treatment in sequence to obtain a carbide; Step 3, mixing the carbide with an activator and performing an activation treatment to obtain the porous carbon material; The activator comprises potassium hydroxide and sodium carbonate, and the mass ratio of the potassium hydroxide to the sodium carbonate is 1:(0.1-0.3); The activation temperature is T 5 ℃, time is t 5 h; 621≤T 5 ≤854; 0.5≤t 5 ≤6.

7. The preparation method according to claim 6, It is characterized in that The preparation method satisfies at least one of the following conditions: (1) The phenolic compound includes at least one of phenol, resorcinol, phloroglucinol, and bisphenol A; (2) The acidic catalyst includes at least one of hydrochloric acid, sulfuric acid, nitric acid, and oxalic acid; (3) the aldehyde compound comprises at least one of formaldehyde, paraformaldehyde, furfural and acetaldehyde; (4) The stabilizer includes at least one of polyvinyl alcohol, polyethylene glycol, hydroxymethyl cellulose, carboxymethyl cellulose, and polyvinyl pyrrolidone; (5) The mass ratio of the phenolic compound to the stabilizer is 1:(0.01-2.8); (6) The temperature of the curing treatment is T 3 ℃, time is t 3 h; 40≤T 3 ≤120; 0.5≤t 3 ≤6; (7) The temperature of the carbonization treatment is T 4 ℃, time is t 4 h; 500≤T 4 ≤1000; 0.5≤t 4 ≤6; (8) The mass ratio of the carbide to the activator is w, 0.1≤w≤1.

8. A silicon-carbon material, It is characterized in that The porous carbon material comprises the porous carbon material according to any one of claims 1 to 5 or the porous carbon material prepared by the preparation method according to claim 6 or 7.

9. A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, It is characterized in that The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector; the negative electrode mixture layer comprises the silicon-carbon material according to claim 8.

10. An electronic device, It is characterized in that The electronic device comprises the secondary battery according to claim 9.

Citation Information

Patent Citations

  • Porous carbon microspheres, preparation method and application thereof, and silicon-carbon negative electrode material

    CN116495731A

  • Silicon-carbon containing electrode material and secondary battery including the same

    US20240128443A1

Cited By

  • Secondary battery and electronic device

    CN119275238A

  • Silicon carbon material and preparation method thereof, secondary battery and electronic device

    CN119920885A

  • Porous carbon material, negative electrode material, negative electrode plate, secondary battery and preparation method of secondary battery

    CN119954155A

  • Porous carbon material, negative electrode material, negative electrode sheet, secondary battery, and method for manufacturing the same

    CN119954155B

  • Porous carbon particle and preparation method thereof, negative electrode active material and lithium ion battery

    CN121394392A