Method for strengthening low-temperature acid leaching of high-purity quartz sand

Through the mixed acid leaching of inorganic acid and short-chain organic acid and microwave ultrasonic synergistic technology, the problems of difficulty in penetration of pickling liquid and high dry energy consumption in the quartz sand purification process are solved, and efficient and low-temperature quartz sand impurity dissolution is achieved. Obtain high-purity quartz sand, simplify the process flow and reduce energy consumption.

CN118929671APending Publication Date: 2024-11-12CENT SOUTH UNIV

Patent Information

Application Number
CN202411090343.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing quartz sand purification process, pickling liquid is difficult to penetrate into the quartz sand particles and has high dry energy consumption, resulting in high production costs and great environmental impact. The traditional acid leaching process requires high temperature pretreatment, the process is complex and resource consumption is high.

Method used

The mixed acid of inorganic acid and short-chain organic acid is used for acid leaching, and the combination of microwave and ultrasound to strengthen the physical contact and chemical reaction between quartz sand and acid, so as to achieve the wet efficient dissolution and removal of impurities components of quartz sand at low temperatures, and construct The acid-leaching system and the dual-field collaborative strengthening system of complex inorganic acid and organic acid.

Benefits of technology

It realizes the dissolution of impurity components of quartz sand with high efficiency, low temperature and low energy consumption, and obtains high-purity quartz sand at level 4N5 or above, simplifies the process flow, reduces energy consumption, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929671A_ABST
    Figure CN118929671A_ABST
Patent Text Reader

Abstract

The invention discloses a method for strengthening low-temperature acid leaching of high-purity quartz sand, which comprises the following steps of: putting a quartz sand raw material and a mixed acid solution into a closed reaction kettle to carry out impurity removal reaction, applying microwave and ultrasonic action to an external field in the reaction process, and washing and deacidifying the obtained product to obtain the high-purity quartz sand with the grade of 4N5 or above, the mixed acid solution comprises inorganic acid and short-chain organic acid. The inorganic acid and the short-chain organic acid are compounded to maintain an acid leaching system at a proper acid concentration, the quartz sand is subjected to efficient and lasting impurity removal, meanwhile, the physical contact and impurity removal reaction of the quartz sand and the mixed acid solution are reinforced through the cooperation of microwaves and ultrasonic waves, and the method has the advantages of being simple in process, high in impurity removal efficiency and the like; the method is easy to popularize and apply in industrial production, and the purity of the quartz sand can be improved to 4N5 or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for quartz sand acid leaching purification, and specifically to a method based on external field synergistically strengthening the physical contact and chemical reaction between quartz sand and acid to achieve low-temperature and efficient removal of impurities, belonging to the field of high-purity processing of non-metallic mineral materials. Background Art

[0002] In the fields of semiconductors, optical fiber communications, lasers, aerospace, etc., high-purity quartz sand, as a vital basic material, plays a cornerstone role in the development of national strategies. However, the original quartz sand contains various types of impurities, such as associated minerals, inclusions, and defects in the lattice structure, which greatly affect its purity and performance.

[0003] Currently, conventional pickling processes usually rely on inorganic acids such as hydrofluoric acid, hydrochloric acid, nitric acid or sulfuric acid for purification. Although these acids can effectively dissolve some impurities, they are also accompanied by significant problems, including strong corrosiveness and poor selective dissolution ability. In addition, most of these processes are operated under normal temperature and electric heating conditions and are carried out in batches in pickling tanks. This method not only leads to large amounts of acid usage and long processing time, thereby increasing production costs, but also makes waste acid treatment a difficult problem. Inefficient heat transfer is also one of the problems, because heat mainly penetrates into the interior of the quartz sand particles gradually through heat conduction, resulting in energy waste.

[0004] Although existing patents such as CN111153409B, CN110950346 A and CN115465866A have proposed acid leaching or microwave-assisted acid leaching of quartz sand, in these processes, the quartz sand first needs to undergo a dry pretreatment step of microwave high-temperature roasting, during which the quartz sand will undergo significant changes in physical and chemical properties. Moreover, the microwave treatment temperature used is generally high, at least 400°C, and even up to 900°C. After such pretreatment, the quartz sand enters the acid leaching stage or ultrasonic acid leaching stage. This two-step independent operation process is both complex and resource-consuming.

[0005] In view of this, it has become particularly urgent to seek a new method to enhance the acid leaching of high-purity quartz sand, which can effectively reduce the environmental impact of quartz processing and improve energy efficiency. Summary of the invention

[0006] In view of the problems that the pickling solution is difficult to penetrate into the interior of the quartz sand particles and the dry method has high energy consumption during the pickling process in the prior art quartz sand purification process, the purpose of the present invention is to provide a method for strengthening the low-temperature acid leaching of high-purity quartz sand. Based on the chemical composition and impurity morphology characteristics of quartz sand, the method uses a mixed acid of inorganic acid and short-chain organic acid for acid leaching, and simultaneously uses microwaves and ultrasound to synergistically strengthen the physical contact and chemical reaction process between quartz sand and acid, so as to achieve the wet method of efficient dissolution and removal of quartz sand impurity components at a lower temperature in one step.

[0007] In order to achieve the above technical objectives, the present invention provides a method for strengthening low-temperature acid leaching of high-purity quartz sand, which method comprises placing a quartz sand raw material and a mixed acid solution in a closed reactor to carry out an impurity removal reaction, and applying microwave and ultrasonic effects in an external field during the reaction process, and the obtained product is washed with water to remove the acid, so as to obtain high-purity quartz sand of grade 4N5 or above; the mixed acid solution comprises an inorganic acid and a short-chain organic acid.

[0008] The key to the technical solution of the present invention is to construct an acid leaching system of a compound of inorganic acid and organic acid to promote the efficient and selective dissolution of impurity components in quartz sand. Existing processes mostly use an inorganic acid system composed of hydrofluoric acid, nitric acid, hydrochloric acid, etc. The above-mentioned inorganic acids have strong acidity and can effectively destroy the composition and structure of associated minerals or coated impurities, causing them to dissolve. However, inorganic acids have poor selectivity, and their dissolution process is indiscriminate dissolution, resulting in the ablation of quartz. The quartz sand acid leaching process is long, and the inorganic acid reaction process is gradually consumed, resulting in a decrease in acidity in the later stage. In particular, after a large amount of surface impurities are dissolved in the initial stage, the driving force for diffusion into the interior of the quartz sand particles to dissolve the coated impurities under subsequent low-acid conditions is greatly reduced. Studies have found that compared with inorganic acids, the process of treating quartz sand with short-chain organic acids, except for H + The chemical bonds between the metal ions and oxygen atoms of the quartz sand impurities are destroyed, and at the same time, there is a ligand-promoted dissolution mechanism, that is, the organic acid radicals selectively complex with inorganic ions such as calcium, iron, and aluminum, reduce the liquid phase saturation index, and selectively promote their dissolution. In addition, during the organic acid treatment process, the hydrolysis of the acid radical ions can maintain the stable acidity of the system for a long time, and has the advantage of strong buffering capacity. However, the process of treating quartz sand with organic acids alone has problems such as slow dissolution rate and low dissolution rate. Therefore, the scheme of the present invention is based on the difference in the physicochemical properties of inorganic acids and organic acids in the quartz sand acid leaching process, and constructs an efficient compound system of the two, giving full play to the advantages of strong acidity and fast dissolution of inorganic acids, strong selectivity of inorganic acids, and strong buffering capacity, to achieve efficient and selective dissolution of impurities in quartz sand.

[0009] Another key to the technical solution of the present invention is to construct a dual external field synergistic strengthening system, that is, microwave heating and ultrasound in the acid leaching process synergistically promote the physical combination and chemical reaction of quartz sand and acid. Increasing the temperature of the acid leaching system can accelerate the reaction between acid and impurities and improve the impurity removal efficiency. Traditional acid leaching uses electric heating, and the heat gradually heats up the inside of the quartz sand through conduction, which has the disadvantages of slow heating speed and low efficiency. Previous studies have found that microwaves have the characteristics of selective heating of quartz sand, the quartz sand matrix has a weak absorption capacity for microwave energy, and the impurity components in the acid solution and quartz sand can better absorb the heat of microwaves, so that the temperature of the quartz sand surface and internal impurity-enriched area rises rapidly, promoting acid dissolution of the quartz sand surface and impurity-enriched area. In the production process, large-scale reaction tanks are generally used for batch production. The accumulation of a large amount of quartz sand will result in less contact between the bottom or internal quartz sand and the acid. The acid leaching process is significantly affected by diffusion. Stirring and other methods can be used to improve the liquid-solid contact effect. However, there is no effective prevention for how to stir a large amount of quartz sand in a high temperature and strong acid system. Metal stirring can cause corrosion and dissolution of the stirring equipment, pollute the quartz sand, and the organic stirring device has limited force and insufficient stirring. Therefore, the present invention constructs an external field strengthening measure of ultrasound and microwave synergy. The quartz sand particles are vibrated at high frequency by microwaves, and a large number of gaps are generated between the particles, which promotes the flow and diffusion of the acid solution between the particles. At the same time, the vibration generated by ultrasound promotes the collision of the quartz sand particles and the acid medium, making their contact more complete and the combination more tight. In addition, the efficient heat source provided by microwaves can activate the cavitation effect of ultrasound, enhance the energy release when the cavitation bubble ruptures, and further increase the local reaction temperature. Therefore, the energy generated by the vibration can be coupled with microwave heating, and the two can synergistically increase the temperature field on the surface of the quartz sand, strengthen the acid immersion water thermal impurity removal reaction process, and significantly reduce the temperature required for the reaction.

[0010] As a preferred solution, the microwave frequency is 433-5800 MHz. The present invention utilizes the difference in wave absorption performance between the quartz sand matrix and the lattice impurities. The microwave can act on the impurities in a directional manner, increase the temperature of the impurities, and accelerate the reaction of the impurities with the mixed acid medium. The magnitude of the microwave frequency can control the heating and temperature rise process of the impurities inside the quartz sand particles and the mixed acid solution, thereby achieving the purpose of regulating the acid dissolution of the impurity components of the quartz sand. If the microwave frequency is too low, the heating rate is too slow, and it is difficult to limit the temperature rise of the impurities inside the quartz sand and the acid reaction site, and the reaction rate is not high.

[0011] As a preferred solution, the power of the ultrasound is 200 to 1800 W. In the quartz sand acid leaching process, the use of ultrasound can avoid the diffusion of the acid medium in the bottom of the reactor and other areas, and effectively improve the contact between the quartz sand and the mixed acid medium. If the ultrasonic power is too high, it will not only cause high process energy consumption, but also cause excessive vibration of solid particles to form an interface layer between the quartz sand and the acid solution, affecting the solid-liquid contact. If the ultrasonic power is too low, it will cause excessive accumulation at the bottom of the reactor or in the middle of the material, and the acid medium cannot effectively penetrate, and it cannot produce a significant synergistic effect with microwaves.

[0012] As a preferred solution, the SiO2 mass content of the quartz sand raw material is ≥99.95%. The quartz sand raw material of the present invention is quartz sand obtained after crushing and sorting quartz minerals such as vein quartz, crystal, pegmatite, quartzite, etc., and its SiO2 mass content is ≥99.95%. If the SiO2 content in the quartz sand is too low, the content of impurity components is high, resulting in a large amount of acid used in the acid leaching process, a long acid leaching time, and reduced operating efficiency. In addition, 99.95% of the quartz sand raw material is easy to obtain in the existing process.

[0013] As a preferred solution, the inorganic acid is at least one of hydrofluoric acid, hydrochloric acid, nitric acid and sulfuric acid.

[0014] As a preferred embodiment, the short-chain organic acid is at least one of acetic acid, propionic acid, butyric acid, oxalic acid and oxalic acid.

[0015] As a preferred solution, the volume concentration of the mixed acid solution is 15-40%; the mixed acid solution is composed of an inorganic acid and a short-chain organic acid in a volume ratio of (1-2): (1-3). In the composite system of short-chain organic acid and inorganic acid of the present invention, when the acid concentration is too low, the reaction rate is slow and the dissolution degree is low during the dissolution of impurity components, thereby affecting the production efficiency and the degree of purification. Although appropriately increasing the acid concentration can accelerate the acid dissolution rate or degree, when the acid concentration is too high, it will obviously lead to the dissolution of quartz particles, increase acid consumption and the difficulty of subsequent acid wastewater treatment. And the control of the volume ratio of inorganic acid and short-chain organic acid in the mixed acid is also relatively important. By controlling the volume ratio of the two, efficient, highly selective and highly durable acid leaching and impurity removal of quartz sand can be achieved. If the amount of inorganic acid is too high, although the impurity components are dissolved quickly due to the strong acidity of the inorganic acid, the quartz sand impurity selectivity is poor and the acidity of the acid leaching process drops significantly. If the amount of inorganic acid is too low, although the advantages of short-chain organic acids such as strong selectivity for impurities and large buffering capacity can be utilized, the overall dissolution rate of the acid leaching process will be low, which will significantly increase the acid leaching time.

[0016] As a preferred solution, the conditions of the impurity removal reaction are: temperature of 45-115°C and time of 1-16h. As the temperature rises, the pressure in the kettle increases. Too high a temperature will cause the pressure in the reactor to be too high, affecting the safe and stable operation of the equipment; too low a temperature will cause the pressure in the reactor to be low, affecting the diffusion of the acid medium into the dense quartz sand particles. The degree of solubility of the impurity components is determined by the reaction rate and reaction time. When the rate is constant, the reaction time is extended, and the total amount of dissolved impurities increases, which is beneficial to the purification effect, but will lead to a decrease in operating efficiency. On the contrary, a large amount of undissolved impurity components will remain in the quartz sand after acid leaching.

[0017] As a preferred solution, the mass ratio of the quartz sand raw material to the mixed acid solution is (0.5-3):1.

[0018] As a preferred solution, the total volume of the quartz sand raw material and the mixed acid solution is less than or equal to 2 / 3 of the total volume of the reactor. Quartz sand acid leaching is carried out in a closed reactor. The increase in pressure in the reactor is related to the amount of material loaded. Too much loading will cause the reactor pressure to be too high, affecting the safe and stable operation of the equipment and bringing certain risks to the safety of the operators. On the contrary, the reactor pressure is low, which affects the diffusion of the mixed acid medium into the dense quartz sand particles.

[0019] After the quartz sand of the present invention is reacted with organic acid and inorganic acid in a reactor by microwave and ultrasonic synergistic strengthening, high-purity quartz sand is obtained after solid-liquid separation, and some acid will remain on its surface. In order to meet the subsequent quartz sand processing and application requirements, it needs to be rinsed with deionized water to near neutrality.

[0020] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0021] 1) The technical solution provided by the present invention is based on the composition and structural characteristics of quartz sand. A mixed acid of short-chain organic acid and inorganic acid is used to maintain the acid leaching system at an appropriate acid concentration, and the quartz sand is efficiently and lastingly removed from impurities. At the same time, microwaves and ultrasound are used in a coordinated manner to strengthen the physical combination and chemical reaction of quartz sand and the mixed acid solution during the acid leaching process, thereby increasing the dissolution rate of impurity components during the acid leaching process, reducing the reaction temperature, and improving the impurity removal effect. The acid leaching removal of quartz sand impurities is achieved quickly and efficiently, and high-purity and ultra-high-purity quartz sand products can be obtained.

[0022] 2) The present invention is a wet reaction system, which does not require high-temperature calcination of quartz sand, has low energy consumption and simple process.

[0023] 3) The method provided by the present invention has the advantages of simple process flow, low temperature and energy consumption, good purification effect, etc. It can quickly and efficiently produce high-purity and ultra-high-purity quartz sand products and is suitable for large-scale industrial production.

[0024] 4) The present invention can comprehensively control the total acid concentration, reaction rate and reaction selectivity of the acid leaching system by controlling the volumes of the inorganic acid and the short-chain organic acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The quartz sand product is prepared by the method for strengthening low-temperature acid leaching of high-purity quartz sand in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner in conjunction with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0027] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0028] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.

[0029] Example 1

[0030] A quartz sand raw material with a SiO2 mass content of 99.95% and a mixed solution of HF and acetic acid are placed in a hydrothermal reactor, with a HF volume concentration of 10% and an acetic acid volume concentration of 5%. The mass ratio of the quartz sand raw material to the mixed acid solution is 1:1, and the filling amount is 2 / 3 of the total volume of the reactor. After sealing, microwave and ultrasound synergistic effects are adopted, with a microwave frequency of 433 MHz, an ultrasonic power of 1600 W, a reaction temperature of 115°C, and a reaction time of 1 h. Afterwards, the sample is digested according to the requirements of the national standard GB / T 32650-2016, and the contents of 13 impurity components are measured, and then the SiO2 content of the product is calculated to be 99.9955%.

[0031] Example 2

[0032] A quartz sand raw material with a SiO2 mass content of 99.97% and a mixed solution of hydrochloric acid and oxalic acid are placed in a hydrothermal reactor, with a hydrochloric acid volume concentration of 10%, an oxalic acid volume concentration of 10%, a mass ratio of the quartz sand raw material to the mixed acid solution of 0.5:1, and a filling amount of 1 / 2 of the total volume of the reactor. After sealing, microwave and ultrasound synergistic effects are adopted, with a microwave frequency of 915 MHz, an ultrasonic power of 1800 W, a reaction temperature of 45°C, and a reaction time of 8 hours. Afterwards, the sample is digested according to the requirements of the national standard GB / T 32650-2016, and the contents of 13 impurity components are measured, and then the SiO2 content of the product is calculated to be 99.9961%.

[0033] Example 3

[0034] A quartz sand raw material with a SiO2 mass content of 99.99% and a mixed solution of hydrofluoric acid, acetic acid and propionic acid are placed in a hydrothermal reactor, with a volume concentration of 10% for hydrofluoric acid, 10% for acetic acid, and 20% for propionic acid. The mass ratio of the quartz sand raw material to the mixed acid solution is 3:1, and the filling amount is 2 / 3 of the total volume of the reactor. After sealing, microwave and ultrasound synergistic effects are adopted, with a microwave frequency of 5800 MHz, an ultrasonic power of 600 W, a reaction temperature of 80°C, and a reaction time of 16 hours. Then, the sample is digested according to the national standard GB / T32650-2016 and the contents of 13 impurity components are measured, and the SiO2 content of the product is calculated to be 99.9974%.

[0035] Example 4

[0036] A quartz sand raw material with a SiO2 mass content of 99.99% and a mixed solution of hydrochloric acid, sulfuric acid and butyric acid are placed in a hydrothermal reactor, with a volume concentration of 10% for hydrochloric acid, 10% for sulfuric acid, and 10% for butyric acid. The mass ratio of the quartz sand raw material to the mixed acid solution is 2:1, and the filling amount is 2 / 3 of the total volume of the reactor. After sealing, microwave and ultrasound synergistic effects are adopted, with a microwave frequency of 2450 MHz, an ultrasonic power of 200 W, a reaction temperature of 110°C, and a reaction time of 9 hours. Afterwards, the sample is digested according to the requirements of the national standard GB / T 32650-2016, and the contents of 13 impurity components are measured, and then the SiO2 content of the product is calculated to be 99.9969%.

[0037] Comparative Example 1

[0038] Compared with Example 1, the only difference is that an equal amount of acetic acid is used as the acid leaching medium for acid leaching, and the other steps and conditions are the same.

[0039] The final acid leaching product has a SiO2 content of 99.962%.

[0040] Comparative Example 2

[0041] Compared with Example 3, the only difference is that electric heating and acid leaching are used (the acid leaching medium is the same as that of Example 3), microwave and ultrasound are not used, and the other steps and conditions are the same.

[0042] The final acid leaching product has a SiO2 content of 99.987%.

[0043] Comparative Example 3

[0044] Compared with Example 4, the only difference is that only microwave, electric heating and acid leaching are used without ultrasound, and the other steps and conditions are the same.

[0045] The final acid leaching product has a SiO2 content of 99.993%.

[0046] Comparative Example 4

[0047] Compared with Example 4, the only difference is that an equal amount of long-chain organic acid hexadecanoic acid is used to replace butyric acid, and the other steps and conditions are the same.

[0048] The final acid leaching product has a SiO2 content of 99.992%.

Claims

1. A method for strengthening low temperature acid leaching of high purity quartz sand, Features: The quartz sand raw material and the mixed acid solution are placed in a closed reactor to undergo an impurity removal reaction, and microwave and ultrasonic effects are applied in the external field during the reaction process. The obtained product is washed with water to remove the acid, thereby obtaining high-purity quartz sand of grade 4N5 or above; The mixed acid solution includes an inorganic acid and a short-chain organic acid; The microwave frequency is 433 MHz to 5800 MHz.

2. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 1, Features: The SiO 2 Quality content ≥99.95%.

3. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 2, Features: The inorganic acid is at least one of hydrofluoric acid, hydrochloric acid, nitric acid and sulfuric acid.

4. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 3, Features: The short-chain organic acid is at least one of acetic acid, propionic acid, butyric acid, oxalic acid and oxalic acid.

5. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 1, 3 or 4, Features: The volume concentration of the mixed acid solution is 15-40%; the mixed acid solution is composed of an inorganic acid and a short-chain organic acid in a volume ratio of (1-2):(1-3).

6. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 5, Features: The conditions of the impurity removal reaction are: temperature of 45 to 115° C. and time of 1 to 16 hours.

7. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 6, Features: The mass ratio of the quartz sand raw material to the mixed acid solution is (0.5-3):

1.

8. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 7, Features: The power of the ultrasound is 200-1800W.

9. A method for strengthening low-temperature acid leaching of high-purity quartz sand according to claim 7, Features: The total volume of the quartz sand raw material and the mixed acid solution is less than or equal to 2 / 3 of the total volume of the reactor.

Citation Information

Patent Citations

  • Process for removing bubble inclusions in quartz sand through microwave acid cleaning

    CN105883817A

  • Preparation method of high-purity quartz sand

    CN111892059A

  • Preparation treatment process for producing high-purity quartz sand

    CN115180624A

  • High-purity quartz sand refining process and high-purity quartz sand

    CN115465866A

Cited By

  • Ultrasonic-assisted acid-saving method for refining quartz sand through multi-step pickling

    CN119771841A