Preparation method and application of Li4SiO4-based granular adsorbent

The preparation of Li4SiO4-based particle adsorbents through one-step molding method solves the problems of low adsorption capacity and complex molding process in low temperature and low CO2 environments, and achieves the performance improvement of efficient CO2 adsorption and long life, which is suitable for industrial applications.

CN118929682APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411092921.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Li4SiO4-based CO2 adsorbent has low adsorption capacity in low temperature and low CO2 concentration environments, complex molding process and high cost, resulting in poor performance and short service life in actual applications.

Method used

The Li4SiO4-based particle adsorbent is prepared by a one-step molding method in a muffle furnace by two-stage calcination method, which simplifies the process and reduces costs, and retains the porous structure and adsorption properties of the particles.

Benefits of technology

It has achieved efficient CO2 adsorption performance in low temperature and low CO2 concentration environment, and has a small loss of adsorption capacity after 150 regenerations, which significantly improves the service life and industrial application potential of Li4SiO4-based particle adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929682A_ABST
    Figure CN118929682A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a Li4SiO4-based granular adsorbent, the method is as follows: lithium salt and silicon-containing ore particles are mixed, the mixture is placed in a muffle furnace for two-stage roasting to obtain the granular Li4SiO4 adsorbent, the Li4SiO4-based granular adsorbent is applied to CO2 adsorption, the adsorption capacity can reach 29.09 wt% under the condition of 600DEG C / 20vol% CO2, and the loss of the adsorption capacity is small after 150 times of cycle tests; the prepared adsorbent particles have the advantages of high thermal stability, abundant pore structures, uniform particle size, good hardness, excellent CO2 adsorption performance, no need of secondary granulation, simple forming process, low cost and facilitation of industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of CO2 adsorbents, and relates to a preparation method of a Li4SiO4-based granular adsorbent and application of the Li4SiO4-based granular adsorbent in CO2 adsorption. Background Art

[0002] Human-caused CO2 emissions, especially CO2 released from fossil fuel combustion, are considered to be one of the main causes of global extreme climate events such as global warming and greenhouse effect. Therefore, the study of high-temperature CO2 adsorbents is the key to the effective development of CCUS technology. Li4SiO4 has the advantages of fast adsorption rate, high adsorption capacity and wide adsorption temperature range, making it an ideal high-temperature CO2 adsorbent.

[0003] However, there are two serious problems with the adsorption performance of Li4SiO4-based CO2 adsorbents: 1) As the CO2 concentration and reaction temperature decrease, the adsorption capacity of Li4SiO4 will deteriorate significantly. For example, when the adsorption temperature is between 650-700 o C and pure CO2 atmosphere, the CO2 adsorption capacity of Li4SiO4 can reach about 35wt%. However, when the temperature is reduced to 600 o When the CO2 concentration is below 20 vol%, the CO2 adsorption capacity of commercial Li4SiO4 is only about 10 wt%. In practical applications, the reaction temperature usually fluctuates greatly, and the CO2 concentration is generally low (10-20 vol%). This also makes it difficult for most Li4SiO4-based CO2 adsorbents to be suitable for industrial applications.

[0004] In addition, in order to meet the needs of practical applications, the molding process is a necessary step. At present, the traditional molding process is to add a binder to the powder material, and shape it by extrusion, spheronization and other methods, and then calcine it again. The mechanical pressure and the use of chemical additives in this process may cause changes in the internal structure of the adsorbent particles, densify the interior of the particles, and then reduce the adsorption capacity and cycle stability of the adsorbent. In order to make the molded material have pores, a pore-forming agent needs to be added. Such methods require secondary granulation of Li4SiO4 powder, which is cumbersome and costly. Summary of the invention

[0005] In order to solve the problems of complex molding process, high cost and low adsorption capacity of Li4SiO4 adsorbent in the prior art, the present invention provides a one-step molding method for preparing a high-performance Li4SiO4-based granular adsorbent.

[0006] The method comprises washing and drying the granular porous silicon-containing ore with water, then uniformly mixing the lithium salt and the dried granular silicon-containing ore, placing the mixture in a muffle furnace, and preparing a Li4SiO4-based granular adsorbent by a two-stage roasting method.

[0007] The lithium salt is LiNO3 with a low melting point, the silicon-containing ore particles have a porous structure, SiO2 content is greater than 40%, and the hardness is greater than 1 N. The silicon-containing ore particles are selected from pumice, perlite, and red jade.

[0008] The molar ratio of Li:Si is 4-6:1.

[0009] Another object of the present invention is to apply the Li4SiO4-based granular adsorbent prepared by the above method to CO2 adsorption.

[0010] Compared with the prior art, the present invention has the following advantages: 1. The Li4SiO4 forming method of the present invention is simple, reliable and low in cost. The method uses silicon-containing ore particles as a substrate and converts them into Li4SiO4 particles in situ through a two-step roasting process, thereby achieving simultaneous completion of Li4SiO4 synthesis and forming. The prepared Li4SiO4 particles have good thermal stability; 2. The Li4SiO4 particles prepared by the present invention exhibit excellent adsorption in CO2 capture applications, especially in low-temperature and low-concentration CO2 environments, and have a long service life; o C) Under low CO2 concentration (20 vol%), the CO2 adsorption performance of the Li4SiO4 particles prepared by the present invention is as high as 29.09 wt%, and the adsorbent has no obvious adsorption capacity loss after 150 regenerations, which is far superior to the traditional high-purity Li4SiO4 powder adsorbent. It meets the actual application needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is a physical picture of the Li4SiO4-based granular adsorbent after synthesis; Figure 2 1 is a schematic diagram of the results of thermogravimetric analysis of the CO2 adsorption performance of the Li4SiO4-based granular adsorbent of Example 1 and the control Li4SiO4; Figure 3 is a schematic diagram of the CO2 adsorption performance results of the Li4SiO4-based granular adsorbent prepared in Example 2; Figure 4 is the test result of the Li4SiO4-based granular adsorbent of Example 2 after 150 cycles; Figure 5 is the test result of the control Li4SiO4 of Example 2 after 30 cycles; Figure 6 is a physical picture of the Li4SiO4-based granular adsorbent after synthesis in Example 3; Figure 7 is a physical picture of the Li4SiO4-based granular adsorbent after synthesis in Example 4; Figure 8 1 is a schematic diagram of the results of the thermogravimetric analysis of the CO2 adsorption performance of the Li4SiO4-based granular adsorbents of Example 3 and Example 4; Fig. 9 It is the test result of the Li4SiO4 based granular adsorbent of Example 3 and Example 4 after 150 cycles. DETAILED DESCRIPTION

[0012] The present invention is further described in detail below in conjunction with embodiments and drawings, but the protection scope of the present invention is not limited to the contents described above. Example 1

[0013] (1) Select pumice particles (SiO2=63.75%, hardness=25.27N) with a particle size of less than 1 cm, immerse them in deionized water, rinse them with deionized water, and then put them in an oven to dry at 60°C; (2) According to the SiO2 content in pumice, according to the molar ratio of Li:Si of 4:1, weigh LiNO3 and pumice particles and put them into an Al2O3 crucible, mix them so that the pumice particles are spread on the bottom of the crucible and the LiNO3 covers the pumice particles; (3) Place the Al2O3 crucible prepared in step (2) into a muffle furnace, calcine at 270°C for 1 h, and then heat to 700°C for 5 h. After calcination, cool to room temperature and take out to obtain a Li4SiO4-based granular adsorbent. The morphology of the adsorbent is shown in FIG. Figure 1 ,As can be seen from the figure, the particles prepared by this method retain the shape of the substance itself, and the particles are relatively uniform.

[0014] At the same time, Li4SiO4 was prepared with high-purity silica powder and LiNO3 as a control. That is, high-purity silica and LiNO3 were fully ground in a mortar with ethanol as the solvent and then dried in an oven with a Li:Si molar ratio of 4:1. They were then poured into an Al2O3 crucible and finally calcined at 700°C in a muffle furnace for 5 hours to obtain control Li4SiO4 as a control.

[0015] The CO2 adsorption performance of the Li4SiO4-based granular adsorbent of this embodiment and the control Li4SiO4 was tested by thermogravimetric analysis. The adsorption conditions were as follows: the temperature was raised to 600°C in a pure N2 atmosphere and maintained for 10 minutes; the temperature was maintained and the gas was switched to 20% CO2 (N2 was the balance gas) and maintained for 120 minutes; the results were as follows: Figure 2As shown, the horizontal axis is the adsorption time, and the vertical axis is the mass percentage of the adsorption amount. It can be seen that in the first 20 minutes, the adsorption rate of the Li4SiO4-based granular adsorbent is fast, and the adsorption amount reaches 18.2wt%. Then the adsorption rate gradually slows down and reaches 22.3wt% at 120 minutes. The adsorption amount of the control Li4SiO4 at 120 minutes is 18.2wt%. The adsorption rate and adsorption capacity are weaker than those of the Li4SiO4-based granular adsorbent ( Figure 2 ). Example 2

[0016] (1) Select pumice particles (SiO2=63.75%, hardness=25.27N) with a particle size of less than 1 cm, immerse them in deionized water, rinse them with deionized water, and then put them in an oven to dry at 60°C; (2) According to the SiO2 content in the pumice, LiNO3 and pumice particles are weighed and placed in an Al2O3 crucible at a Li:Si molar ratio of 4:1, 5:1 and 6:1, and the pumice particles are spread on the bottom of the crucible and the LiNO3 is covered on the pumice particles in a mixed manner; (3) The Al2O3 crucible prepared in step (2) was placed in a muffle furnace, first calcined at 270°C for 1 hour, then heated to 700°C and calcined for 5 hours; after calcination, the crucible was cooled to room temperature and taken out to obtain a Li4SiO4-based granular adsorbent.

[0017] The method for testing the CO2 adsorption performance of the Li4SiO4-based granular adsorbent in this embodiment is the same as that in Example 1. The results are shown in Figure 3 It can be seen from the figure that when the molar ratio of Li:Si is 5:1, the adsorption rate of the Li4SiO4-based granular adsorbent is the fastest, and the adsorption amount reaches 20.1wt% at 20min, and then the adsorption rate gradually slows down, reaching 25.7wt% at 120min; when the molar ratio of Li:Si is 6:1, the adsorption amount reaches 13.9wt% at 20min, and reaches 20wt% at 120min; when the molar ratio of Li:Si is 4:1, the adsorption amount reaches 18.2wt% at 20min, and reaches 22.3wt% at 120min.

[0018] In order to further explore the adsorption performance of the Li4SiO4-based granular adsorbent, the Li4SiO4-based granular adsorbent with a molar ratio of Li:Si of 5:1 in Example 2 was subjected to a cyclic test. The adsorption conditions were: adsorption temperature 600°C, holding time 30 min, atmosphere 20% CO2 (N2 as the balance gas); desorption conditions were: desorption temperature 600°C, holding time 10 min, atmosphere pure N2. The results are as follows: Figure 4As shown, the horizontal axis is the number of adsorption-desorption cycles, and the vertical axis is the adsorption amount. At the same time, Li4SiO4 was prepared from high-purity silicon dioxide powder and LiNO3 as a control (the preparation method is shown in Example 1, and the test method is the same as above).

[0019] from Figure 4 It can be seen that the adsorbent has the highest adsorption capacity in the first cycle, reaching 19.7wt%, and only loses 1.8wt% after 150 cycles. Figure 5 It can be seen that the adsorption capacity of the control Li4SiO4 drops sharply with the increase of the number of cycles, and the adsorption capacity is only 4.3wt% after 30 cycles. Example 3

[0020] (1) Select perlite particles (SiO2=74.31%, hardness=22.49N) with a particle size of less than 1 cm, immerse them in deionized water, rinse them with deionized water, and then put them in an oven to dry at 60°C; (2) According to the SiO2 content in the perlite, at a molar ratio of Li:Si of 5:1, weigh LiNO3 and perlite particles and put them into an Al2O3 crucible, mix them so that the perlite particles are spread on the bottom of the crucible and the LiNO3 covers the perlite particles; (3) The Al2O3 crucible prepared in step (2) was placed in a muffle furnace, first calcined at 270°C for 1 hour, then heated to 700°C and calcined for 5 hours; after calcination, it was cooled to room temperature and taken out to obtain the Li4SiO4-based granular adsorbent ( Figure 6 ); The method for testing the CO2 adsorption performance of Li4SiO4-based granular adsorbent is the same as in Example 1, and the results are shown in Figure 8 As can be seen from the figure, at 20 minutes, the adsorption amount of the Li4SiO4-based granular adsorbent of this embodiment is 22.31wt%, and then the adsorption rate gradually slows down, and the adsorption amount is 29.09wt% at 120 minutes. Example 4

[0021] (1) Select Akadama particles (SiO2=45.90%, hardness=13.50N) with a particle size of less than 1 cm, sieve them, and then put them into an oven to dry at 60°C; (2) According to the SiO2 content in Akadama, LiNO3 and Akadama particles were weighed and placed in an Al2O3 crucible at a Li:Si molar ratio of 5:1, and the Akadama particles were spread on the bottom of the crucible and LiNO3 was covered on the Akadama particles; (3) The Al2O3 crucible prepared in step (2) was placed in a muffle furnace, first calcined at 270°C for 1 hour, then heated to 700°C and calcined for 5 hours; after calcination, it was cooled to room temperature and taken out to obtain the Li4SiO4-based granular adsorbent ( Figure 7); The method for testing the CO2 adsorption performance of Li4SiO4-based granular adsorbent is the same as in Example 1, and the results are shown in Figure 8 As can be seen from the figure, at 20 minutes, the adsorption amount of the Li4SiO4-based granular adsorbent of this embodiment is 15.72wt%, and then the adsorption rate gradually slows down, and the adsorption amount is 21.07wt% at 120 minutes.

[0022] In order to further explore the adsorption performance of the Li4SiO4-based granular adsorbent, the Li4SiO4-based granular adsorbent of Example 3 and Example 4 was subjected to a cyclic test. The adsorption conditions were: adsorption temperature 600°C, insulation time 30 min, and atmosphere of 20% CO2 (N2 as the balance gas); the desorption conditions were: desorption temperature 600°C, insulation time 10 min, and atmosphere of pure N2.

[0023] The results are as follows Fig. 9 As shown, the horizontal axis is the number of adsorption-desorption cycles, and the vertical axis is the adsorption amount. It can be seen from the figure that the adsorbent prepared in Example 3 has the highest adsorption capacity in the first cycle, reaching 21.16wt%; then it decreases rapidly, and then gradually increases after the 10th cycle, and then tends to be flat, and stabilizes at 19.79wt% after 150 cycles. The adsorbent prepared in Example 4 shows an overall stable trend, and the adsorption capacity only loses 1.36wt% after 150 cycles.

[0024] The above results show that the Li4SiO4-based granular adsorbent prepared by the method of the present invention is superior to the control Li4SiO4 in terms of adsorption performance and cycle performance. At the same time, compared with the control Li4SiO4, the preparation process of the Li4SiO4-based granular adsorbent prepared by the present invention is simple, the powder molding process is reduced, and the industrial continuous production and application are greatly facilitated, providing a good development prospect for the practical application of Li4SiO4.

Claims

1. A method for preparing a Li4SiO4-based granular adsorbent, characterized in that: The lithium salt is mixed with silicon-containing ore particles, the mixture is placed in a muffle furnace, and the Li4SiO4-based granular adsorbent is prepared by a two-stage roasting method.

2. The method for preparing the Li4SiO4-based granular adsorbent according to claim 1, characterized in that: The silicon-containing ore particles have a porous structure, SiO2 content>40%, and hardness greater than 1 N.

3. The method for preparing the Li4SiO4-based granular adsorbent according to claim 1, characterized in that: Lithium salts are fusible and have a melting point below 500 o C.

4. The method for preparing the Li4SiO4-based granular adsorbent according to claim 1, characterized in that: In the two-stage calcination method, the first stage calcination temperature is the melting temperature of the lithium salt, the calcination time is 30min-5h, and the second stage calcination temperature is 600-800 o C, calcination time 1-5h.

5. The method for preparing the Li4SiO4-based granular adsorbent according to claim 1, characterized in that: The molar ratio of Li:Si is 4-6:

1.

6. Use of the Li4SiO4-based granular adsorbent prepared by the preparation method of the Li4SiO4-based granular adsorbent according to any one of claims 1 to 6 in CO2 adsorption.

Citation Information

Patent Citations

  • Method for preparing lithium silicate material for absorbing CO2 at high temperature

    CN101653718A

  • Preparation method of lithium-based carbon dioxide adsorbent

    CN102908981A

  • Method for preparing lithium silicate high-temperature carbon sequestration material by means of serpentine ore residues after magnesium extracting

    CN104003412A

  • Lithium-based CO2 adsorbing agent and preparing method thereof

    CN109621891A

  • Absorbent for carbon dioxide, useful for promoting carbon monoxide shift conversion, comprises a lithium silicate that has been doped and / or thermally / chemically pretreated

    DE102004030513A1