Preparation method and application of superfine calcined kaolin with low oil absorption value
By wet re-grinding and spray drying during the preparation process of calcined kaolin, combined with sodium hexametaphosphate dispersant, the problem of high oil absorption value and fineness after calcination was solved, and low oil absorption value and high fineness were obtained Kaolin, suitable for rubber reinforcement, improves dispersion performance and reinforcement.
Patent Information
- Application Number
- CN202411113427.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
The problems of increased oil absorption value and thicker fineness of calcined kaolin lead to difficulties in dispersion and reduced reinforcement performance when reinforcing rubber.
The preparation method of calcined kaolin clay with low oil absorption value includes crushing, wet coarse grinding and ultrafine grinding, centrifugal spray drying, depolymerization and dispersion , and then calcined in an internal heat calcination rotary kiln, and after calcination, wet re-grinding and spray-drying, using sodium hexametaphosphate as a dispersant, oil absorption value and particle size are controlled.
Kaolin with low oil absorption value and high fineness after calcination has been achieved, with better dispersion performance and reinforcement, suitable for rubber materials, reducing vulcanization time and dust pollution.
Smart Images

Figure BDA0004992952690000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of calcined kaolin, in particular to a preparation method and application of ultrafine calcined kaolin with low oil absorption value. Background Art
[0002] Oil absorption value is one of the important indicators of calcined kaolin. It reflects the specific surface area, particle size and agglomeration degree of the product to a certain extent. Generally, the finer the particle size and the larger the specific surface area, the higher the oil absorption value. The oil absorption value also has a great influence on the application performance of the product. Taking coating as an example, the oil absorption value of 4000 mesh calcined kaolin is preferably 55-60g / 100g. At this time, it can show better hiding power and less resin and additive adsorption. Calcined kaolin with high oil absorption value can bring better ink adsorption performance when used for thermal paper. Calcined kaolin can also be used for rubber reinforcement. Compared with uncalcined kaolin, calcined kaolin has high whiteness and better insulation, so it has a certain application market. After calcination, the oil absorption value of kaolin will be significantly increased. For example, the oil absorption value of kaolin with a fineness of -2μm90% is about 45g / 100g before calcination, but after calcination, the fineness is reduced to about -2μm80%, while the oil absorption value increases to 60-70. Due to the obvious increase in oil absorption value, calcined kaolin will cause dispersion difficulties when used in rubber, and the fineness becomes coarser after calcination, which will reduce the reinforcing performance of the product. Summary of the invention
[0003] The invention provides a preparation method and application of ultrafine calcined kaolin with low oil absorption value, so as to solve the technical problem that the oil absorption value of calcined kaolin increases, the fineness becomes coarser, and the reinforcing performance is reduced when used for rubber reinforcement.
[0004] According to one aspect of the present invention, there is provided a method for preparing ultrafine calcined kaolin with low oil absorption value, comprising the following steps:
[0005] (1) crushing and wet-grinding kaolinite white ore, kaolinite gangue and purple wood knot ore into slurry, then wet-grinding into slurry with a particle size of more than 90% of -2 μm, and then centrifugally classifying to remove coarse particles into ultrafine slurry;
[0006] (2) drying the ultrafine slurry into powder by centrifugal spray drying, then deagglomerating the agglomerated powder into ultrafine powder by a deagglomerator, and then transporting the powder to a silo by air flow;
[0007] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcining rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. to form calcined powder;
[0008] (4) adding water and a dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 40% to 50%, and then grinding it into an ultrafine slurry by a stirring mill;
[0009] (5) The ultrafine slurry is spray-dried to obtain ultrafine calcined kaolin with low oil absorption value.
[0010] Furthermore, in the step (1), the amounts of kaolinite white ore, kaolinite gangue and purple wood knot ore are: 3-5 parts of kaolinite white ore, 2-6 parts of kaolinite gangue and 5-9 parts of purple wood knot ore.
[0011] Furthermore, the ultrafine slurry in step (2) is centrifugally spray-dried into a powder with a moisture content of less than 5%.
[0012] Furthermore, the calcination time in step (3) is 0.5 to 1.5 hours.
[0013] Furthermore, in the step (4), the amount of the dispersant used is 0.1-0.3%, and the dispersant is sodium hexametaphosphate.
[0014] Furthermore, the ultrafine slurry in step (4) has a particle size of -2 μm or more, a blue light whiteness of more than 90%, and passes through a 325-mesh sieve with a sieve residue of less than 0.005%.
[0015] Furthermore, in the step (4), the flow rate of the slurry entering and exiting the grinding machine when grinding with a stirred mill is 4.5 to 5 m / s. 3 / h.
[0016] Furthermore, the spray drying temperature in step (4) is 300°C to 450°C.
[0017] According to another aspect of the present invention, there is also provided an ultrafine calcined kaolin with low oil absorption value, which is prepared by the above method. The ultrafine calcined kaolin with low oil absorption value has an oil absorption value ≤50g / 100g, a whiteness ≥90%, and a particle size of -2μm ≥90%.
[0018] According to another aspect of the present invention, there is also provided an application of ultrafine calcined kaolin with low oil absorption value, wherein the kaolin is used as a reinforcing filler in rubber materials.
[0019] The present invention has the following beneficial effects:
[0020] (1) The present invention further wet-mixes the calcined kaolin, deagglomerates and grinds it with a stirring mill, fully eliminates the adhesion of particles during the calcination process, makes the product finer, and largely eliminates the particle gaps increased by adhesion. The particle size distribution is close to that before calcination, thereby improving the product fineness and reducing the oil absorption value. The obtained low oil absorption value ultrafine calcined kaolin product is microspherical, and compared with the existing powdered calcined kaolin products, it has a larger bulk density, is easier to disperse during rubber refining, does not cause dust pollution, and has a shorter vulcanization time.
[0021] (2) The low oil absorption ultrafine calcined kaolin prepared by the present invention has an oil absorption value of ≤50g / 100g, a whiteness of ≥90%, and a particle size of -2μm ≥90%. When used in rubber materials, it has better reinforcement and dispersion properties and meets market demand. DETAILED DESCRIPTION
[0022] The following is a detailed description of the embodiments of the present invention, but the present invention can be implemented in many different ways as defined and covered below.
[0023] The embodiment of the first aspect of the present invention provides a method for preparing ultrafine calcined kaolin with low oil absorption value, comprising the following steps:
[0024] (1) crushing and wet-grinding kaolinite white ore, kaolinite gangue and purple wood knot ore into a slurry of about 200 mesh, and then wet-grinding into a slurry with a particle size of more than 90% of -2 μm, and then centrifugally classifying and removing coarse particles to obtain an ultrafine slurry with a particle size of more than 95% of -2 μm and a concentration of 40% to 50%;
[0025] (2) centrifugally spray drying the ultrafine slurry at a temperature of 300° C. to 450° C. into powder, and then using a deagglomerator to deagglomerate the powder particles generated during drying to break them up into ultrafine powder, which is then transported to a silo via air flow;
[0026] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcining rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. for about 1 hour to form a calcined powder with a blue light whiteness of ≥ 90%;
[0027] (4) adding water and a dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 40% to 50%, and then grinding it into an ultrafine slurry by a stirring mill;
[0028] (5) The ultrafine slurry is spray-dried at a high temperature fan frequency of 33 (Hz) to obtain ultrafine calcined kaolin with low oil absorption value.
[0029] The current common calcined kaolin production process is: ore-crushing-wet coarse grinding-wet fine grinding-centrifugal spray drying-depolymerization-calcination-depolymerization-packaging. The ore is crushed into particles less than 30mm by a jaw crusher, and then enters the dry grinding equipment to be coarsely ground to less than 325 mesh. That is, the raw ore is crushed into particles less than 5mm by a hammer crusher and then enters a dry ball mill for coarse grinding to less than 325 meshes, and then water and dispersant are added to the slurry preparation tank to prepare a slurry with a solid content of (48-52%), which is then pumped to the ultrafine grinding equipment for ultrafine grinding to become an ultrafine slurry with a particle size less than 2 microns (μm) and greater than 92%. The ultrafine slurry is dried to become a powder, and the powder is dispersed by a depolymerization device to break up the powder agglomerated due to drying to become an ultrafine powder. The dispersed ultrafine powder enters the calcination system for calcination to become a calcined material, and the calcined material is cooled and then the powder agglomerated due to calcination is broken up by a depolymerization device to become an ultrafine finished product powder, which is finally packaged as a finished product. This calcined kaolin is difficult to have the characteristics of high fineness and low oil absorption value at the same time.
[0030] The process route of the present invention is: raw material - crushing - wet coarse grinding - wet fine grinding - centrifugal classification - centrifugal spray drying - depolymerization - calcination - slurry preparation - wet fine grinding - spray drying - packaging. Based on the existing process route, the present invention changes from depolymerization after calcination, changes dry depolymerization to wet re-grinding plus spray drying, no depolymerization after spray drying, and the product is in the form of microspheres.
[0031] Preliminary studies have shown that calcination will cause a loss in the fineness of kaolin products, even if the particle size becomes coarser. The reason is that during calcination, low-melting-point substances on the surface of the particles, such as potassium and sodium, will cause kaolin to adhere, thereby making the particles coarser and causing larger particle gaps. The oil absorption value is directly related to the size of the particle gaps. The larger the particle gaps, the higher the oil absorption value. In the slurry of wet ultrafine grinding before calcination, the large and small particles are evenly distributed and well graded, the gaps between the particles are small, and the oil absorption value is low. During calcination, a large number of gaps between particles are created after the decomposition and oxidation of structural water, carbon and organic matter to discharge gas, thereby increasing the oil absorption value. The present invention uses wet re-grinding after calcination to fill large and small particles with each other and eliminate the gaps between particles, thereby reducing the oil absorption value; at the same time, ultrafine grinding is performed after calcination to decompose the particle agglomeration caused by calcination, reduce the particle size of the material particles, and increase the fineness. Re-grinding after calcination is to restore the particle size loss caused by calcination so that the product has high fineness.
[0032] The present invention wet-mixes the calcined kaolin, deagglomerates and grinds it with a stirring mill, fully eliminates the adhesion of particles during the calcination process, makes the product finer, eliminates the particle gaps increased by adhesion to a great extent, and makes the particle size distribution close to that before calcination, thereby improving the product fineness and reducing the oil absorption value at the same time; the obtained ultrafine calcined kaolin product with low oil absorption value is in the shape of microspheres.
[0033] In an embodiment of the present invention, the amount of kaolinite white ore, kaolinite gangue and purple wood knot ore in step (1) is: 3-5 parts of kaolinite white ore, 2-6 parts of kaolinite gangue and 5-9 parts of purple wood knot ore. Kaolinite white ore and kaolinite gangue need to be sieved to remove powder.
[0034] Preferably, the weight proportion of the kaolinite white ore can be 3, 4 or 5; the weight proportion of the kaolinite gangue can be 2, 3, 4, 5 or 6; the weight proportion of the purple wood knot ore can be 5, 6, 7, 8 or 9. The raw ore can be a combination of any weight proportions of the above components.
[0035] Preferably, 3 parts of kaolinite white ore, 2 parts of kaolinite gangue, and 5 parts of purple wood knot ore.
[0036] The kaolinite white ore used in the present invention has an aluminum oxide content of 32% to 37%, a silicon oxide content of 46% to 50%, and a loss on ignition of 12% to 15%. The kaolinite white ore does not contain carbon and organic matter, which is beneficial to reducing the porosity formed by the decomposition of carbon and organic matter, thereby reducing the oil absorption value; the kaolinite gangue has an aluminum oxide content of 30% to 35%, a silicon oxide content of 48% to 52%, a carbon and organic matter content of 2% to 3%, and a loss on ignition of 16% to 19%. Since it contains a small amount of carbon and organic matter (the carbon and organic matter content in black ore has little effect on the oil absorption value), it is beneficial to form a weak reducing atmosphere during the calcination process, so that the high-valent iron oxide impurities in the material with a dark color are reduced to low-valent ferrous oxide with a light color, thereby improving the whiteness of the kaolin. The aluminum oxide content in the purple wood knot ore is 30% to 34%, and the silicon oxide content is 34% to 38%. Its aluminum oxide content is relatively high, easy to grind, and beneficial to filling the gaps between the material particles, thereby reducing the oil absorption value.
[0037] In an embodiment of the present invention, the ultrafine slurry in step (2) is centrifugally spray-dried into a powder with a moisture content of less than 5%.
[0038] In an embodiment of the present invention, in step (3), the temperature of the combustion chamber of the calcining kiln is 1100-1200°C, the temperature inside the calcining kiln is 1050-1100°C, the calcining time is 0.5-1.5h, and the ultrafine powder is calcined into a calcined powder with a blue light whiteness ≥90%.
[0039] In the embodiment of the present invention, the amount of dispersant used in step (4) is 0.1-0.3%, and the dispersant is sodium hexametaphosphate. The amount of dispersant used is determined to be 0.1-0.3% by experiments, and the dispersion effect is measured by reducing the viscosity of the slurry. The slurry concentration of 40%-50% is also determined by experiments that the slurry viscosity is in the optimal range. If the concentration is too high, the viscosity is high and the grinding effect is poor. If the concentration is too low, the moisture is high, which affects the subsequent drying efficiency and cost.
[0040] In the embodiment of the present invention, the ultrafine slurry obtained by wet grinding in step (4) has a particle size of -2 μm or more, a blue light whiteness of more than 90%, and a sieve residue of less than 0.005% after passing through a 325-mesh sieve. Furthermore, in step (4), the flow rate of the slurry entering and exiting the grinding machine when grinding with a stirred mill is 4.5 to 5 m / s. 3 / h, wet regrinding is to increase fineness and reduce oil absorption value.
[0041] Furthermore, the temperature of the spray drying in step (4) is 300° C. to 450° C. Spray drying only dries out the water, and does not generate interparticle gaps due to the decomposition of carbon and organic matter during calcination, and does not affect the oil absorption value of the product.
[0042] According to another aspect of the present invention, there is also provided an ultrafine calcined kaolin with low oil absorption value, which is prepared by the above method. The ultrafine calcined kaolin with low oil absorption value has an oil absorption value ≤50g / 100g, a whiteness ≥90%, and a particle size of -2μm ≥90%.
[0043] According to another aspect of the present invention, there is also provided an application of ultrafine calcined kaolin with low oil absorption value, wherein the kaolin is used as a reinforcing filler in rubber materials.
[0044] The ultrafine calcined kaolin with low oil absorption value prepared by the present invention is used in styrene-butadiene rubber as a reinforcing filler to replace white carbon black. The specific formula is: 100 parts of SBR, 50 parts of kaolin, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of polyethylene glycol, 2 parts of sulfur, 1.2 parts of accelerator MBTS, 0.7 parts of accelerator MBT, and 0.5 parts of accelerator D.
[0045] Test results of rubber performance indicators: tensile strength 28.1MP, elongation at break 561%, tear strength 100kN / m, compression heat generation 47°C.
[0046] If the oil absorption value of kaolin is high, it means that the kaolin particles can absorb more rubber materials, making it more difficult to disperse during mixing, while increasing the amount of rubber materials used, which is not conducive to reducing costs; therefore, kaolin used for rubber reinforcement should have a low oil absorption value.
[0047] According to the test results, replacing white carbon black with kaolin can reduce the mixing energy consumption of the rubber compound by 10% to 15%, the Mooney viscosity of the mixed rubber can be reduced by more than 10 Mooney values, the tensile strength can be improved, and the compression heat generation can be reduced by 2 to 4°C.
[0048] Example 1
[0049] This embodiment provides a method for preparing ultrafine calcined kaolin with low oil absorption value, comprising the following steps:
[0050] (1) The raw ore is crushed and wet-grinded into a 200-mesh slurry, and then wet-milled into a slurry with a particle size of more than 90% of -2 μm. The coarse particles are then centrifuged to remove the coarse particles to obtain an ultrafine slurry with a particle size of more than 95% of -2 μm and a concentration of 45%;
[0051] (2) centrifugally spray drying the ultrafine slurry at a temperature of 300° C. to 450° C. into a powder with a moisture content of less than 5%, and then using a deagglomerator to deagglomerate the powder particles generated during drying to break them up into ultrafine powder, which is then transported to a silo via air flow;
[0052] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcining rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. for about 0.5 h to form a calcined powder with a blue light whiteness of ≥ 90%;
[0053] (4) adding water and 0.2% of a dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 45%, and then grinding it with a stirring mill to form an ultrafine slurry with a particle size of more than 90% of -2 μm, a blue light whiteness of more than 90%, and a 325 mesh residue of less than 0.005%;
[0054] (5) The ultrafine slurry is spray-dried with a high-temperature blower to a moisture content of less than 5%, thereby obtaining ultrafine calcined kaolin with a low oil absorption value.
[0055] Example 2
[0056] This embodiment provides a method for preparing ultrafine calcined kaolin with low oil absorption value, comprising the following steps:
[0057] (1) The raw ore is crushed and wet-grinded into a 220-mesh slurry, and then wet-milled into a slurry with a particle size of more than 90% of -2 μm. The coarse particles are then centrifuged to remove the coarse particles to obtain an ultrafine slurry with a particle size of more than 95% of -2 μm and a concentration of 50%;
[0058] (2) centrifugally spray drying the ultrafine slurry at a temperature of 300° C. to 450° C. into a powder with a moisture content of less than 5%, and then using a deagglomerator to deagglomerate the powder particles generated during drying to break them up into ultrafine powder, which is then transported to a silo via air flow;
[0059] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcination rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. for 1 hour to form a calcined powder with a blue light whiteness of ≥ 90%;
[0060] (4) adding water and 0.1% dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 50%, and then grinding it with a stirring mill to form an ultrafine slurry with a particle size of more than 90% of -2 μm, a blue light whiteness of more than 90%, and a 325 mesh residue of less than 0.005%;
[0061] (5) The ultrafine slurry is spray-dried with a high-temperature blower to a moisture content of less than 5%, thereby obtaining ultrafine calcined kaolin with a low oil absorption value.
[0062] Example 3
[0063] This embodiment provides a method for preparing ultrafine calcined kaolin with low oil absorption value, comprising the following steps:
[0064] (1) The raw ore is crushed and wet-grinded into a 180-mesh slurry, and then wet-milled into a slurry with a particle size of more than 90% of -2 μm. The coarse particles are then centrifuged to remove the coarse particles to obtain an ultrafine slurry with a particle size of more than 95% of -2 μm and a concentration of 40%;
[0065] (2) centrifugally spray drying the ultrafine slurry at a temperature of 300° C. to 450° C. into a powder with a moisture content of less than 5%, and then using a deagglomerator to deagglomerate the powder particles generated during drying to break them up into ultrafine powder, which is then transported to a silo via air flow;
[0066] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcination rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. for 1.5 hours to form a calcined powder with a blue light whiteness of ≥ 90%;
[0067] (4) adding water and 0.3% dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 40%, and then grinding it with a stirring mill to form an ultrafine slurry with a particle size of more than 90% -2 μm, a blue light whiteness of more than 90%, and a 325 mesh residue of less than 0.005%;
[0068] (5) The ultrafine slurry is spray-dried with a high-temperature blower to a moisture content of less than 5%, thereby obtaining ultrafine calcined kaolin with a low oil absorption value.
[0069] Example 4
[0070] This embodiment provides a method for preparing ultrafine calcined kaolin with low oil absorption value, comprising the following steps:
[0071] (1) The raw ore is crushed and wet-grinded into a 200-mesh slurry, and then wet-milled into a slurry with a particle size of more than 90% of -2 μm. The coarse particles are then centrifuged to remove the coarse particles to obtain an ultrafine slurry with a particle size of more than 95% of -2 μm and a concentration of 42%;
[0072] (2) centrifugally spray drying the ultrafine slurry at a temperature of 300° C. to 450° C. into a powder with a moisture content of less than 5%, and then using a deagglomerator to deagglomerate the powder particles generated during drying to break them up into ultrafine powder, which is then transported to a silo via air flow;
[0073] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcination rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. for 1 hour to form a calcined powder with a blue light whiteness of ≥ 90%;
[0074] (4) adding water and 0.2% of a dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 42%, and then grinding it with a stirring mill to form an ultrafine slurry with a particle size of more than 90% of -2 μm, a blue light whiteness of more than 90%, and a 325 mesh residue of less than 0.005%;
[0075] (5) The ultrafine slurry is spray-dried with a high-temperature blower to a moisture content of less than 5%, thereby obtaining ultrafine calcined kaolin with a low oil absorption value.
[0076] Comparative Example 1
[0077] A method for preparing calcined kaolin comprises the following steps:
[0078] (1) The raw ore is crushed and wet-grinded into a 200-mesh slurry, and then wet-milled into a slurry with a particle size of more than 90% of -2 μm. The coarse particles are then centrifuged to remove the coarse particles to obtain an ultrafine slurry with a particle size of more than 95% of -2 μm and a concentration of 42%;
[0079] (2) centrifugally spray drying the ultrafine slurry at a temperature of 300° C. to 450° C. into a powder with a moisture content of less than 5%, and then using a deagglomerator to deagglomerate the powder particles generated during drying to break them up into ultrafine powder, which is then transported to a silo via air flow;
[0080] (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcination rotary kiln via a screw conveyor, and calcined at a temperature of 1050° C. to 1100° C. for 1 hour to form a calcined powder with a blue light whiteness of ≥ 90%;
[0081] (4) Packing the calcined powder.
[0082] According to GB / T 14563-2020 Kaolin and its test methods, the kaolin products obtained in the above Examples 1-4 and Comparative Example 1 were sampled and the test results are shown in Table 1:
[0083] Table 1 Kaolin test results in Examples 1-4 and Comparative Example 1
[0084]
[0085] According to the above table, in Examples 1-4, on the basis of Comparative Example 1 of the prior art, the process steps of - slurry preparation - wet fine grinding - spray drying are performed after calcining the kaolin. After calcining, wet grinding is performed again to fill the large and small particles with each other, eliminate the gaps between the particles, and thus reduce the oil absorption value; at the same time, ultrafine grinding is performed after calcining to decompose the particle agglomeration caused by calcination of the material, reduce the particle size of the material particles, and improve the fineness; after spray drying, there is no depolymerization. The spray drying of the present invention only dries and removes the water, and does not produce the particle gaps formed by the decomposition of carbon and organic matter during calcination, which does not affect the oil absorption value of the product. The product particles after spray drying are in the form of microspheres. Therefore, kaolin with both lower oil absorption value and higher whiteness can be obtained.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing ultrafine calcined kaolin with low oil absorption value, characterized in that: The following steps are involved: (1) crushing and wet-grinding kaolinite white ore, kaolinite gangue and purple wood knot ore into slurry, then wet-grinding into slurry by ultrafine grinding, and then centrifugally classifying to remove coarse particles into ultrafine slurry; (2) drying the ultrafine slurry into powder by centrifugal spray drying, then deagglomerating the agglomerated powder into ultrafine powder by a deagglomerator, and then conveying it to a silo by air flow; (3) The ultrafine powder is uniformly and continuously fed into an internal heating calcining rotary kiln via a screw conveyor to be calcined into calcined powder; (4) adding water and a dispersant to the calcined powder, stirring and dispersing to form a slurry with a concentration of 40% to 50%, and then grinding it into an ultrafine slurry by a stirring mill; (5) The ultrafine slurry is spray-dried to obtain ultrafine calcined kaolin with low oil absorption value.
2. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: In the step (1), the dosage of kaolinite white ore, kaolinite gangue and purple wood knot ore is: 3-5 parts of kaolinite white ore, 2-6 parts of kaolinite gangue and 5-9 parts of purple wood knot ore.
3. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: In the step (2), the ultrafine slurry is dried by centrifugal spraying to form a powder with a moisture content of less than 5%.
4. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: In the step (3), the calcination temperature is 1050-1110° C., and the calcination time is 0.5-1.5 h.
5. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: The amount of dispersant used in step (4) is 0.1-0.3%, and the dispersant is sodium hexametaphosphate.
6. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: The ultrafine slurry in step (4) has a particle size of more than 90% of -2 μm, a blue light whiteness of more than 90%, passes through a 325-mesh sieve, and the residue on the sieve is less than 0.005%.
7. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: In the step (4), the flow rate of the slurry entering and leaving the grinding machine when grinding with a stirred mill is 4.5 to 5 m 3 / h.
8. The method for preparing ultrafine calcined kaolin with low oil absorption value according to claim 1, characterized in that: The spray drying temperature in step (4) is 300°C to 450°C.
9. An ultrafine calcined kaolin with low oil absorption value, characterized in that: The ultrafine calcined kaolin with low oil absorption value is prepared by the method described in any one of claims 1 to 8. The ultrafine calcined kaolin with low oil absorption value has an oil absorption value of ≤50g / 100g, a whiteness of ≥90%, and a particle size of -2μm ≥90%.
10. An application of ultrafine calcined kaolin with low oil absorption value, characterized in that: The kaolin is used as a reinforcing filler in rubber materials.
Citation Information
Patent Citations
Surface modification method of titanium dioxide-PCC mixed filling material
CN102733255A
Coal-series kaolin gas suspension calcination method
CN102795633A
Production method for ultrafine low-conductivity calcined kaolin
CN105000570A
Preparation method of calcined kaolin with high whiteness and ultrahigh oil absorption
CN110577225A
Production method of calcined kaolin for glass fibers
CN111533440A