Purification method of electronic-grade ammonium salt

Through concentrated solution crystallization, redissolution and dehydration treatment, the problems of slow spontaneous nucleation rate and uneven dispersion in ammonium salt purification were solved, and high purity and high uniformity ammonium salt crystal generation was achieved, suitable for electronic grade ammonium salts. The production reduces the metal impurity content and production costs.

CN118929691AActive Publication Date: 2024-11-12HUBEI SINOPHORUS ELECTRONIC MATERIALS CO LTD

Patent Information

Application Number
CN202410863763.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-11-12
Estimated Expiration
2044-06-29

AI Technical Summary

Technical Problem

The prior art has problems such as slow spontaneous nucleation and crystallization rate, difficult solution precipitation, uneven crystal dispersion, metal impurities storage, and crystallization water are prone to moisture during the purification process of ammonium salt, resulting in high metal content and low purity in the product, and purification process High energy consumption and high cost.

Method used

The purity and uniformity of the ammonium salt are gradually improved by ultrapure water dissolution, cooling and crystallization, repeated washing, centrifugation, addition of liquid seeds, dehydrating agent treatment and vacuum drying, and the purity and uniformity of the ammonium salt are reduced by reducing the content of metal impurities.

Benefits of technology

High uniform crystal formation of ammonium salts has been achieved, the metal content has been reduced to less than 1 ppb, and the purity of ammonium salts has reached more than 99%. It is suitable for the precision field and reduces production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929691A_ABST
    Figure CN118929691A_ABST
Patent Text Reader

Abstract

The invention relates to a purification method of electronic-grade ammonium salt. Firstly, industrial-grade ammonium salt is used for crystallization, and then the industrial-grade ammonium salt is used for preparing seed crystals which are highly uniformly distributed in a liquid state. Preparing industrial-grade ammonium salt into a concentrated solution, cooling to a certain degree, adding seed crystals, continuously cooling to a target temperature to separate out crystals, and heating to 10 DEG C at a speed of 2min / DEG C; and finally, adding a dehydrating agent into the crystal in a turning state, heating to 15 DEG C, and spin-drying and drying to obtain a target product. According to the method, the seed crystal adding mode and the following steps of cooling, heating and the like are greatly different from those of a traditional process, the steps of solution crystallization, two-step melt crystallization and the like are coupled, different industrial-grade ammonium salts are taken as raw materials, and finally, the content of each metal is 1t; the ammonium salt purity is gt; 99% of electronic-grade ammonium salt can be applied to various high-end fields with harsh requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ammonium salt purification, and particularly relates to a method for purifying electronic grade ammonium salt. Background Art Ammonium salts refer to salt compounds containing ammonium ions (NH4+). Common ammonium salts include ammonium chloride, ammonium nitrate, ammonium sulfate, ammonium acetate, etc. Ammonium salts have many uses and are widely used in the fields of chemical, pharmaceutical and food.

[0002] In the chemical industry, ammonium salts are widely used. Ammonium chloride is an important chemical raw material and is often used to prepare other ammonium salts and organic compounds. For example, ammonium chloride can be used to prepare ammonium sulfate by reacting with sulfuric acid, and ammonium nitrate can also be prepared by reacting ammonium chloride with nitric acid. In addition, ammonium salts can also be used in the manufacture of batteries, metal corrosion inhibitors, and leather degreasing agents. In the pharmaceutical field, ammonium salts also have some important applications. Ammonium sulfate can be used as an auxiliary preparation to improve the solubility and stability of drugs. Ammonium chloride can be used to prepare ammonia precursors, which is an important solvent and drug ingredient in pharmaceuticals. In addition, ammonium salts can also be used as auxiliary materials for cremation and vacuum casting, used to control flame temperature and reduce metal oxidation, as well as solvents and solvent powders for aluminum alloys, and to prepare smoke screens and smoke control equipment.

[0003] Industrial-grade ammonium salts contain a large amount of Fe, Ca, and Na (>500 ppb), which will greatly limit their scope of use in some precision fields. At present, the commonly used purification technologies for preparing electronic-grade products at home and abroad mainly include rectification, distillation, sublimation, resin exchange, membrane treatment, crystallization and other technologies. Different purification technologies are suitable for the purification process of different products. For technologies such as nanofiltration, resin exchange and membrane treatment, their purification effect and the service life of the equipment often have certain requirements on the viscosity of the required purified product, which requires the ammonium salt to be configured as a dilute solution for use. However, the purified solution contains a large amount of water, which makes it unsuitable for many fields, and its concentration will increase energy consumption and production costs.

[0004] The growth rate of spontaneous nucleation crystallization is slow, and it is easy to cause the solution to be unable to precipitate even when it is in a saturated state, and its yield is low. The added seed crystals are often added in solid form. Due to their extremely uneven dispersion in the solution, the difference in the time of crystal growth and precipitation can easily lead to the crystals entrapping metal impurities, resulting in excessive metal content in the product. In addition, the ammonium acetate crystals themselves will also have some crystal water and are very susceptible to moisture. Conventional dehydrating agents are likely to cause residues on their surfaces. Summary of the invention

[0005] The object of the present invention is to provide a method for purifying electronic grade ammonium salt, wherein a seed crystal with high uniformity is obtained by crystallization and redissolution of a concentrated solution, and then the seed crystal is added to a new concentrated solution to obtain pure crystals. Subsequently, a dehydrating agent is used to dehydrate the crystals, the temperature is raised to make the crystals sweat, and the crystals are dried to obtain an electronic grade ammonium salt with a metal content of less than 1 ppb and an ammonium salt purity greater than 99%. In order to achieve the purpose of the invention, the present invention adopts the following technical solutions: The present invention provides a method for purifying an electronic grade ammonium salt, and the preparation method comprises the following steps: Step 1: Dissolve industrial-grade ammonium salt in ultrapure water, heat and stir to prepare a supersaturated ammonium salt solution; Step 2: Cooling the solution in step 1 to obtain ammonium salt crystals; Step 3: Use a coarse filter bag and ultrapure water mist to repeatedly wash and filter the crystals in step 2 to obtain pure ammonium salt crystals, and then add ultrapure water to prevent them from being completely dissolved; Step 4: Mix well and centrifuge, take the centrifuged liquid as seed crystal, and keep warm; Step 5: Take industrial-grade ammonium salt and prepare a saturated solution with ultrapure water, heat and stir until it is completely dissolved and then cool down; Step 6: adding the liquid seed crystals obtained in step 4 to the solution obtained in step 6; Step 7: Continue to cool down to the target temperature, then heat up again; Step 8: Add a dehydrating agent to the crystals obtained in step 7 while the crystals are being turned over, raise the temperature, and spin dry; Step 9: Place the dried crystals in a vacuum rotary drying oven to dry. The mass solubility of the ammonium salt solution in step 1 is 45%-85%, and the temperature is raised to 25-70°C at 2-5°C / min, preferably to 60, 70, 80, 90°C until dissolved. This means that no large crystals are precipitated to the bottom, but the solution still contains a large number of microcrystals. Cooling can cause spontaneous crystallization, which can be monitored by the PCM system.

[0006] In step 2, the solution is cooled to 22-27°C at a rate of 15-25 min / °C to obtain ammonium salt crystals. Preferably, the solution is cooled to 25°C at a rate of 20 min / °C to obtain ammonium salt crystals. A slow cooling rate and a small temperature difference in step 2 will reduce the yield, but the purpose of this process is to spontaneously grow high-purity seed crystals.

[0007] The crystals washed repeatedly in step 3 have high purity, and the mass of ultrapure water added again is 25%-40% of the mass of the crystals, preferably 25%, 30%, 35%, 40%. The purpose of making the crystals fail to completely dissolve is to allow the liquid to contain ammonium salts for use as seed crystals.

[0008] In step 4, centrifuge after mixing, take the centrifugal liquid as a seed, the grain growth can be made more uniform, because the seed is too large will lead to uneven dispersion, the purpose of centrifugation is to settle large particles, the centrifugal speed is 100-500 r / min, preferably 100, 200, 300 r / min. The insulation temperature is 25-40 ° C. Centrifugation can obtain high uniformity, distributed in the liquid seed, and because it has been repeatedly washed, the seed purity is extremely high at this time, and as a seed, the grain growth can be made more uniform. The purpose of insulation is to prevent the seed from dissolving and spontaneous crystallization. It has been experimentally verified that high metal content can accelerate the precipitation of seed crystals, and ultrapure ammonium salts are used to dissolve and then cool down to form a supersaturated solution, and no crystals are precipitated when the temperature is lowered.

[0009] In step 5, the mass concentration of the saturated ammonium salt solution is 40-80%, the heating end point is 50-100°C, the cooling rate is 5-10 min / °C, and the cooling end point is 20-40°C.

[0010] From a mechanistic point of view, the slower the cooling rate, the better the crystal morphology and purity, but too slow a cooling rate will reduce production efficiency and increase costs. Therefore, it is very important to choose a moderate cooling rate.

[0011] In step six, the amount of liquid seed added is 0.5-2.8% of the mass of the solute, preferably 0.7%, 1.4%, 2.1%, 2.8%.

[0012] The reason for adding seed crystals is to induce growth and balance the supersaturation of the solution system. When the amount of crystals added is too small, the supersaturation in the solution is insufficient. After the amount of crystals added reaches a certain proportion, the state is basically stable, and continuing to add seed crystals will cause waste. When the size of the added seed crystals is too large, they are easy to sink to the bottom, resulting in poor surface morphology uniformity. If the seed crystal size is too small, it is not easy to continue to grow on its surface.

[0013] In step seven, the cooling rate is 10-30 min / °C, the cooling end point is 5°C, and then the temperature is increased to 10°C at a rate of 2 min / °C.

[0014] The establishment of the end point of temperature rise and fall is determined by the characteristics of the ammonium salt solubility curve, where the ratio of concentration difference to temperature difference is the largest and the yield is high. The subsequent temperature rise process is to make the crystals sweat, dissolve the crystals that have been nucleated but not grown, melt and separate some of the adhered crystals, and remove the contained mother liquor.

[0015] The dehydrating agent in step eight is one or more of acetone, N-methylpyrrolidone, furanone, n-butanol, tert-butanol, 1,4-dioxane, and propylene glycol, preferably acetone, N-methylpyrrolidone, n-butanol, tert-butanol, and 1,4-dioxane.

[0016] The addition of dehydrating agent can effectively combine the adsorption and binding water on the surface of the crystal. Heating the crystal again to make it sweat is to remove impurities in the deep layer and remove the residual dehydrating agent. Then it is dried to remove moisture and impurities.

[0017] In step eight, the temperature is raised to 13-17°C at 0.5-1.5 min / °C; Preferably, in step eight, the temperature is raised to 15°C at a rate of 1 min / °C.

[0018] Compared with the prior art, the present invention has the following beneficial effects: 1) The present invention directly configures the product into a saturated solution with a higher concentration, which can enrich the metal impurities more quickly; 2) The seed crystals of the present invention are generated by crystallization of the original solution itself and are added in liquid form, which greatly reduces the cost and the uniformity of subsequent product crystallization, and greatly improves the yield and purity of the product; 3) The coupling of solution crystallization and melt crystallization significantly reduces the metal ion content in the product; 4) Dehydrating agent removes moisture from the product to make it suitable for various precision fields; 5) The operation process is simple and the required equipment is easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Product image of electronic grade ammonium salt of Example 1; Figure 2 Product picture of comparative example 1. DETAILED DESCRIPTION

[0020] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The metal ion concentrations in the four different ammonium salt raw materials used in Examples 1 to 13 of the present invention are shown in Table 1. The metal ion concentrations in the ammonium salt raw materials were tested by ICP-MS spectrometer, and the unit is ppb.

[0021] Table 1 Metal ion concentration of industrial grade ammonium salt raw materials

[0022] Examples 1-13 A method for purifying an ammonium salt of the present invention comprises the following steps: Step 1: Prepare the ammonium salt raw material into a saturated ammonium salt solution with a concentration of 45-85%, and heat it to 60, 70, 80, 90°C at 2-5°C / min until it dissolves. Step 2: Cooling the solution in step 1 to 25°C at a rate of 20 min / °C to obtain ammonium salt crystals; Step 3: Repeatedly wash and filter the crystals in step 2, and add ultrapure water again at a mass of 25, 30, 35, and 40% of the mass of the crystals, which cannot be completely dissolved; Step 4: Mix well and centrifuge at 100, 200, and 300 r / min, take the clear solution, and keep it at 25-40°C; Step 5: prepare the ammonium salt raw material into a saturated ammonium salt solution, the heating end point is 50-100°C, the cooling rate is 5-10 min / °C, and the cooling end point is 20-40°C; Step 6: adding 0.7, 1.4, 2.1, 2.8% of the mass of the solute to the solution in step 5; Step 7: Continue cooling at a rate of 10-30 min / °C, with the cooling end point being 5°C, then heat to 10°C at a rate of 2 min / °C, and wash and filter the resulting crystals; Step 8: spraying the crystals obtained in step 7 with one or more of acetone, N-methylpyrrolidone, n-butanol, tert-butanol, and 1,4-dioxane while turning them over, then heating to 15°C at a rate of 1 min / °C, and drying; Step nine: Place the dried crystals in a vacuum rotary drying oven and dry them at a temperature of 15-30°C for 1-4 hours.

[0023] Table 2 shows the different ammonium salt concentrations, heating conditions, pure water addition amounts, rotation speeds and insulation temperatures for implementing steps 1 to 4 in Examples 1-13; and the heating and cooling conditions, seed addition amounts, continued cooling conditions, dehydrating agent types and vacuum drying conditions for implementing steps 5 to 9.

[0024] Table 2 Process conditions

[0025] The metal contents of the electronic grade ammonium salts prepared under the above conditions were reduced to below 1 ppb, and the purity was greater than 99%. The specific data are shown in Table 3.

[0026] Comparative Example 1: The steps of preparing seed crystals from step 1 to step 4 and adding seed crystals in step 6 of Example 1 were omitted, and saturated ammonium salt solution was directly used for crystallization. At this time, the metal ion content of the product was greater than 1 ppb, which did not meet the requirements of electronic grade ammonium salt. The specific data are shown in Table 3. Compared with Comparative Example 1, the finished product was grayer in color and had poorer uniformity. Figure 2 shown.

[0027] Comparative Example 2: The seed preparation steps of steps 1 to 4 in Example 1 were omitted, and the addition of liquid seeds in step 6 was replaced by adding solid electronic grade ammonium salt. Other conditions remained unchanged. At this time, the metal ion content of the product was qualified, but the final product yield was 90% of that in Example 1.

[0028] Comparative Example 3: Based on Example 1, the amount of pure water added was replaced with 60%, and other conditions remained unchanged. At this time, the metal ion content of the product was greater than 1 ppb, which did not meet the requirements of electronic grade ammonium salts. The specific data are shown in Table 3.

[0029] Comparative Example 4: Based on Example 1, the rotation speed was replaced with 1000 r / min, and other conditions remained unchanged. At this time, the metal ion content of the product was greater than 1 ppb, which did not meet the requirements of electronic grade ammonium salts. The specific data are shown in Table 3.

[0030] Comparative Example 5: Based on Example 1, the insulation temperature was replaced with 60°C, and other conditions remained unchanged. At this time, the metal ion content of the product was greater than 1 ppb, which did not meet the requirements of electronic grade ammonium salts. The specific data are shown in Table 3.

[0031] Comparative Example 6: Based on Example 1, the end point of the saturated solution heating was replaced with 60°C. At this time, the metal ion content of the product was greater than 1 ppb, which did not meet the requirements of electronic grade ammonium salts. The specific data are shown in Table 3.

[0032] Comparative Example 7: Based on Example 1, the cooling rate of the saturated solution was replaced with 5°C / min. At this time, the metal ion content of the product was greater than 1 ppb, which did not meet the requirements of electronic grade ammonium salts. The specific data are shown in Table 3.

[0033] Comparative Example 8: Based on Example 1, no dehydrating agent was added. At this time, the purity of the product was <96%, which did not meet the requirements of electronic grade ammonium salt. The specific data are shown in Table 3.

[0034] It can be seen from Example 1 and Comparative Example 1 that after pre-seeding, the crystals grow more uniformly, have better dispersion and lower metal impurity content. This may be because the added seeds cross an energy barrier to form crystal nuclei, which promotes the rapid and orderly growth of crystals and reduces the generation of fine crystals, so the probability of metal impurities being hidden between crystals is also greatly reduced.

[0035] It can be known from Example 1 and Comparative Example 2 that the added liquid crystal seeds, under the same crystallization conditions, are compared with the electronic-grade solid ammonium salt with lower metal content, in addition to being cheaper, can also improve the production capacity of the final product. This may be because the crystal growth process is greatly affected by fluid mechanics conditions and mass transfer process, the position of the crystal seed addition point should be selected in the region with the best fluid mixing effect, and the direct addition of solid crystal seeds may cause inconsistent saturation in local areas, and the produced tiny crystals penetrate the filter bag during washing, resulting in a reduction in yield. In addition, the direct input of solids has the possibility of bursting crystals. In addition, it was found during the experiment that the metal impurities in the solution can promote the further growth of crystals, and the crystal surface area is small, so it is more stable during washing, and the phenomenon that its impurity metal and ammonium salt do not have eutectic allows it to be removed during subsequent temperature rise.

[0036] It can be seen from Example 1 and Comparative Example 3 that too high a rotation speed will result in unqualified metal content in the product, which may be due to the seed crystal. The particle size distribution of the seed crystal directly affects the particle size distribution of the final product. It is generally believed that the seed crystal should have a narrower particle size distribution. In other words, the particle size of the seed crystal is relatively uniform. Too fast a rotation speed will cause the crystal sedimentation rate in the suspension to be too fast, and the saturation of the resulting seed crystal will be too low. Too slow a rotation speed will result in more large particles and uneven particle size. The seed crystal obtained by the rotation speed of Example 1 is better in both saturation and particle size.

[0037] The temperature of the seed insulation and the temperature of the heating end point of the solution provide a temperature difference, so that a part of the seed surface is slightly dissolved, and the metal wrapped between the crystals can be effectively removed, so as to avoid the formation of eutectics with the ammonium salt in the solution as a crystal nucleus. Insufficient heating temperature will cause some crystals to be unable to dissolve, and a bad crystallization center will be formed in the subsequent cooling process, and there is also the risk of nuclear explosion, which will cause the product metal impurities to be unqualified. In theory, the slower the cooling rate, the higher the purity of the obtained product crystal, but it will undoubtedly lead to an increase in time cost. The cooling rate and cooling end point selected in Example 1 are all based on the premise that the metal content meets the standard. According to the saturation curve and actual operation, the process route is selected with the lowest energy consumption, theoretical yield and actual output.

[0038] Table 3

[0039] The technical solution of the present invention is explained through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above specific embodiments to be implemented. Any improvements made by technicians in the relevant field based on the present invention, or equivalent replacement of the materials selected by the present invention, etc., fall within the scope of protection of the patent.

Claims

1. A method for purifying electronic grade ammonium salt, characterized in that: The etching solution includes the following components by mass percentage: The preparation method steps are as follows: Step 1: Dissolve industrial-grade ammonium salt in ultrapure water, heat and stir to prepare a supersaturated ammonium salt solution; Step 2: Cooling the solution in step 1 to obtain ammonium salt crystals; Step 3: Use a coarse filter bag and ultrapure water mist to repeatedly wash and filter the crystals in step 2 to obtain pure ammonium salt crystals, and then add ultrapure water to partially dissolve them; Step 4: Mix well and centrifuge, take the centrifuge liquid as seed crystal, and keep warm; Step 5: Take industrial-grade ammonium salt and prepare a saturated solution with ultrapure water, heat and stir until it is completely dissolved and then cool down; Step 6: adding the liquid seed crystals obtained in step 4 to the solution obtained in step 6; Step 7: Continue to cool down to the target temperature, then heat up again; Step 8: Add a dehydrating agent to the crystals obtained in step 7 while the crystals are being turned over, raise the temperature, and spin dry; Step 9: Place the dried crystals in a vacuum rotary drying oven to dry.

2. The method for purifying electronic grade ammonium salt according to claim 1, wherein The mass concentration of the supersaturated ammonium salt solution in step 1 is 45-85%, and the temperature is raised to 60-110°C at 2-5°C / min, preferably 60, 70, 80, 90°C until dissolved; In step 2, the solution is cooled to 22-27°C at a rate of 15-25 min / °C to obtain ammonium salt crystals. Preferably, the solution is cooled to 25°C at a rate of 20 min / °C to obtain ammonium salt crystals.

3. The method for purifying electronic grade ammonium salt according to claim 1, wherein In step 3, the amount of ultrapure water added is 25%-40% of the mass of the crystal, preferably 25%, 30%, 35%, 40%.

4. The method for purifying electronic grade ammonium salt according to claim 1, wherein In step 4, the centrifugal speed is 100-500 r / min, preferably 100, 200, 300 r / min, and the insulation temperature is 25-40°C.

5. The method for purifying electronic grade ammonium salt according to claim 1, wherein In step 5, the mass concentration of the saturated solution of ammonium salt is 40-80%, the heating end point is 50-100°C, the cooling rate is 5-10min / °C, and the cooling end point is 20-40°C.

6. The method for purifying electronic grade ammonium salt according to claim 1, wherein In step six, the amount of liquid seed added is 0.5-2.8% of the solid content, preferably 0.7%, 1.4%, 2.1%, 2.8%.

7. The method for purifying electronic grade ammonium salt according to claim 1, wherein In step 7, the cooling rate is 10-30 min / °C, the cooling target temperature is 3-7°C, and then the temperature is increased to 8-12°C at a rate of 1.5-2.5 min / °C; Preferably, the target temperature for cooling is 5°C, and then the temperature is increased to 10°C at a rate of 2 min / °C.

8. The method for purifying electronic grade ammonium salt according to claim 1, wherein The dehydrating agent in step eight is one or more of acetone, N-methylpyrrolidone, furanone, n-butanol, tert-butanol, 1,4-dioxane, and propylene glycol, preferably acetone, N-methylpyrrolidone, n-butanol, tert-butanol, and 1,4-dioxane; In step eight, the temperature is raised to 13-17°C at 0.5-1.5 min / °C; Preferably, the temperature is increased to 15°C at a rate of 1 min / °C.

9. The method for purifying electronic grade ammonium salt according to claim 1, wherein In step nine, the vacuum rotary drying temperature is 15-30° C. and the time is 1-4 h.

10. The electronic grade ammonium salt purified by the method according to any one of claims 1 to 9, characterized in that: The content of each metal in electronic grade ammonium salt is reduced to below 1 ppb, and the purity of ammonium salt is >99%.

Citation Information

Patent Citations

  • Method for producing high-purity ammonium chloride from industrial-grade ammonium chloride

    CN112142068A

  • Industrial production method of electronic pure ammonium sulfite

    CN115353121A

  • Method for removing chloride ions in ammonium sulfate

    CN117602643A

  • Production of ammonium sulfate crystal

    JP2000226211A

  • Inflatable clothing

    KR102870192B1

Cited By

  • Preparation method of electronic-grade ammonium acetate

    CN119798071A

  • Process for the preparation of electronic grade ammonium acetate

    CN119798071B