Preparation method of cerium oxide powder polishing material
Cerium oxide powder polishing material was prepared by combining anti-solvent crystallization precipitation and pulsed electric field heating, which solved the problem of insufficient performance of existing polishing materials and achieved a highly efficient silicon wafer surface polishing effect.
Patent Information
- Application Number
- CN202410982278.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies struggle to produce high-performance cerium oxide polishing materials with sub-nanometer particle sizes and nano-sized internal crystals, resulting in poor polishing effects on silicon wafer surfaces and failing to meet the nano-scale surface accuracy and sub-nanometer surface roughness requirements of ultra-large-scale integrated circuits.
A method combining anti-solvent crystallization precipitation with pulsed electric field heating was used to prepare spherical cerium nitrate crystal particles using cerium nitrate hexahydrate as raw material. These particles were then heated and decomposed under a pulsed electric field to form cerium nitrate powder particles. Finally, nanoscale high-performance cerium oxide powder polishing material was obtained by calcination at 1500℃.
It significantly improved the consumption of polishing slurry, the removal rate of polishing materials, and the surface roughness. The nanoscale surface accuracy and surface roughness quality of silicon wafers were improved by more than double on average.
Smart Images

Figure CN118929731A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polishing material manufacturing, and in particular to a method for preparing a high-performance cerium oxide powder polishing material by combining an anti-solvent crystallization precipitation method with pulse electric field heating. Background Art
[0002] In recent years, with the development of ultra-large-scale integrated circuit technology in the semiconductor field, the wiring of silicon wafer substrates has become increasingly complex and miniaturized, which requires that the surface of the silicon wafer must have nanometer-level surface accuracy and sub-nanometer surface roughness. For this reason, it is necessary to use high-performance polishing materials with sub-nanometer particle size and nanometer-level crystals inside the particles to finely polish the surface of the silicon wafer. At present, the main material that can meet the polishing requirements of the above-mentioned ultra-large-scale integrated circuit boards is cerium oxide (CeO2), which has a series of advantages such as fast polishing speed, high finish and long service life.
[0003] At present, the methods for preparing cerium oxide polishing materials mainly include hydrothermal method, precipitation method, solvent thermal method, sol-gel method and microemulsion method, etc. Utilizing the above methods, although cerium oxide polishing materials can be prepared, they are mainly low-grade products, and high-grade cerium oxide polishing materials with high performance are currently almost entirely dependent on imports. With the development and rapid development of ultra-large-scale integrated circuits in the semiconductor field of my country, the demand for high-performance cerium oxide polishing materials is increasing rapidly. In order to improve the manufacturing level of related products in the semiconductor field of my country as soon as possible and solve the short board problem of ultra-large-scale integrated circuit board polishing materials in my country, it is very urgent to develop high-performance cerium oxide polishing materials. Summary of the invention
[0004] In order to overcome the shortcomings and defects of the current existing technologies and process methods in the process of preparing high-performance cerium oxide powder polishing materials, the present invention proposes a method for preparing high-performance cerium oxide powder polishing materials by combining an anti-solvent crystallization precipitation method with a pulse electric field induction.
[0005] The method for preparing a cerium oxide powder polishing material of the present invention is characterized in that cerium nitrate hexahydrate is used as a raw material, and a high-performance cerium oxide powder polishing material is prepared by combining an anti-solvent crystallization precipitation method and a pulse electric field heating method, and the process steps are as follows:
[0006] 1) Preparation of spherical particles of cerium nitrate hexahydrate; dissolving the cerium nitrate hexahydrate in ethanol to prepare an ethanol cerium nitrate solution with a cerium nitrate concentration of 5 ml / L-20 ml / L, atomizing the ethanol cerium nitrate solution into droplets using an atomizer and spraying the droplets into the ether solution, so that the cerium nitrate hexahydrate is completely precipitated in the ether-ethanol solution and forms spherical cerium nitrate crystal particles; the volume ratio of ether to ethanol in the ether-ethanol solution formed after the cerium nitrate hexahydrate is completely precipitated is 1:1.
[0007] 2) adding 8 g / L-12 g / L of the phenolic resin to the ether-ethanol solution used to generate the spherical cerium nitrate crystal particles, stirring and dissolving and evaporating the solution, removing the ethanol and ether in the solution, allowing the phenolic resin to precipitate and evenly coat the surface of the spherical cerium nitrate crystal particles, and then drying.
[0008] 3) Pulse electric field heating is used to decompose the dried spherical cerium nitrate crystal particles to prepare cerium nitrate powder particles.
[0009] 4) further calcining the cerium nitrate powder particles to remove the carbon coating on the surface of the cerium nitrate powder particles and strengthen the crystal structure thereof, and finally obtaining a nano-scale high-performance cerium oxide powder polishing material.
[0010] The present invention is also characterized in that the ethanol cerium nitrate solution is atomized into droplets at a rate of 100ml / min-200ml / min by an atomizer and sprayed into the ether solution. The ether solution is stirred at a rate of 60rpm. The evaporation of the phenolic resin refers to evaporation at 90°C. The drying temperature of the spherical cerium nitrate crystal particles is 50°C-60°C, and the drying time is about 12h.
[0011] Furthermore, the pulse electric field heating temperature of the present invention is 390°C-410°C, the heating time is about 60 minutes, and the intensity of the pulse electric field is 100V / mm-300V / mm. The pulse electric field heating temperature process of the present invention is:
[0012] The electric furnace was heated at a heating rate of 2℃-3℃ / min. When the temperature reached about 96℃, a pulse electrostatic field was applied to the sample in the furnace with an electric field strength of 200V / mm. At the same time, the furnace temperature was maintained at this temperature for 30min. After the insulation was completed, the electric furnace was heated to 400℃ at a heating rate of 2℃-3℃ / min. After being maintained at 400℃ for 60min, the electric field was unloaded and the sample in the furnace was cooled to room temperature along with the furnace.
[0013] The calcination of the present invention is to place the cerium nitrate powder particles in a crucible, and then place the crucible in an electric furnace, heat it to 1400° C.-1500° C. and keep it warm for 60 minutes.
[0014] The nanometer-level high-performance cerium oxide powder polishing material of the present invention is a nanometer-level particle crystal with a diameter of 1 μm to 3 μm and a cubic structure, and has an obvious directional crystal orientation.
[0015] The invention adopts hexahydrate cerium nitrate as raw material, firstly prepares spherical cerium nitrate crystal particles by anti-solvent crystallization precipitation method, then heats and decomposes under pulse electric field induction to generate cerium nitrate powder particles, and finally calcines at 1500°C to obtain a high-performance cerium oxide powder polishing material with uniform particle size distribution, particle diameter of 1μm to 3μm, and nano-level particle crystals in the particles presenting a cubic structure and obvious directional crystal orientation. The significant advantages and effects of the invention are that, compared with the cerium oxide powder prepared by the conventional method, when the cerium oxide powder polishing material of the invention is used, the consumption of the polishing liquid is not only significantly reduced, but also the material removal rate (MRR) and material removal depth during polishing are respectively increased by 85%-86% and 47%-47.5%, the pits and scratches on the microscopic surface are significantly reduced, and the line roughness Ra and the surface roughness Sa are respectively increased by 51%-52% and 48-49%. Through the nano-level fine polishing of the invention, the nano-level surface shape accuracy and surface roughness quality of the silicon wafer surface are increased by more than double on average. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic flow diagram of the anti-solvent crystallization precipitation method of the present invention;
[0017] Figure 2 It is a schematic diagram of the process of the pulse electric field heating method of the present invention;
[0018] Figure 3 It is an electron microscope photograph of an embodiment of the present invention, showing the particle size of cerium oxide powder and the particle crystal structure inside the particle. DETAILED DESCRIPTION
[0019] The following are exemplary embodiments of the present invention and detailed descriptions of specific embodiments of the present invention. In order to clearly illustrate the present invention, the area range in the drawings may be enlarged or exaggerated, or some graphic structures may not be shown when the text description is clear and concise, and these preferred embodiments are not intended to limit other embodiments of the present invention.
[0020] The technical improvement idea of the present invention is that as a high-performance polishing material, the prepared cerium oxide powder polishing material should have the following necessary properties at the same time: (1) the powder particles are spherical; (2) the particle size distribution is uniform and the dispersion is good; (3) the crystal particles in the particles are nanometer-level; (4) the particles have good crystallinity and have a clear directional crystal orientation. However, based on the current technology and process, it is difficult to prepare a cerium oxide powder material that meets the above properties at the same time.
[0021] In order to achieve the above-mentioned performance, the present invention adopts improvements, uses cerium nitrate hexahydrate as raw material, first prepares spherical particles of cerium nitrate hexahydrate by an anti-solvent crystallization precipitation method, then heats and decomposes them under the induction of a pulse electric field to generate cerium oxide powder particles, and finally calcines them at about 1500°C to obtain a high-performance cerium oxide powder polishing material with uniform particle size distribution, a particle diameter of 1μm to 3μm, a cubic structure of nano-scale particle crystals in the particles, and a clear directional crystal orientation.
[0022] The method for preparing the cerium oxide powder polishing material of the present invention is to prepare the high-performance cerium oxide powder polishing material by combining the atomized anti-solvent crystallization precipitation method and the pulse electric field heating method, and adopts cerium nitrate hexahydrate; ethanol solution; ether solution; phenolic resin and other main materials; and has the following process steps:
[0023] 1) Preparation of spherical particles of cerium nitrate hexahydrate: dissolving the cerium nitrate hexahydrate in ethanol, using ethanol to dissolve the cerium nitrate hexahydrate to form an ethanol cerium nitrate solution, preparing an ethanol cerium nitrate solution with a cerium nitrate concentration of 5ml / L-20ml / L, and then using an atomizer to atomize the ethanol cerium nitrate solution into tiny droplets at a rate of 100ml / min-200ml / min and spraying it into an ether solution stirred at a rate of 60rpm; since the ethanol component in the ethanol cerium nitrate solution is infinitely miscible with ether, the ethanol in the droplets sprayed into the ether solution will separate from the droplets and dissolve into ether to form an ether ethanol solution, while the cerium nitrate hexahydrate is insoluble in ether, so the cerium nitrate hexahydrate is completely precipitated in the ether ethanol solution and forms spherical cerium nitrate crystal particles. The volume ratio of ether to ethanol in the ether ethanol solution formed after the cerium nitrate hexahydrate is completely precipitated is 1:1.
[0024] 2) Add 8g / L-12g / L of the phenolic resin to the ether-ethanol solution for generating spherical cerium nitrate crystal particles, stir and dissolve it thoroughly, and make it evenly dissolved in the ether-ethanol solution; evaporate the phenolic resin at 90°C to remove the ethanol and ether in the solution, and separate the hexahydrate cerium nitrate crystal particles. At this time, the dissolved phenolic resin will gradually precipitate and form a phenolic resin coating on the surface of the spherical cerium nitrate crystal particles, which will wrap the spherical cerium nitrate crystal particles, keep the shape of the spherical cerium nitrate crystal particles unchanged, and prevent the particles from sticking to each other during the subsequent heating and decomposition process. The phenolic resin precipitates and is evenly coated on the surface of the spherical cerium nitrate crystal particles, and then is dried at a drying temperature of 50°C-60°C for about 12 hours.
[0025] 3) The dried spherical cerium nitrate crystal particles are heated and decomposed at 400° C. under the induction of a pulse electric field. During the heating process, the cerium nitrate in the spherical cerium nitrate crystal particles first melts to form a molten salt, and the cerium nitrate particles are oriented under the induction of the pulse electric field. The crystallization process of the cerium nitrate crystal particles is controlled by the pulse electric field parameters to decompose them into cerium nitrate powder particles.
[0026] 4) further calcining the cerium nitrate powder particles, placing the cerium nitrate powder particles in a corundum crucible, and then placing the crucible in an electric furnace and heating it to 1400°C-1500°C and keeping it warm for 60 minutes to remove the carbon coating on the surface of the cerium nitrate powder particles and strengthen its crystal structure, and finally obtaining a nano-scale high-performance cerium oxide powder polishing material with uniform particle size distribution, a diameter of 1μm to 3μm, a cubic structure of nano-scale particle crystals in the particles, and obvious directional crystal orientation.
[0027] In this embodiment, the pulse electric field heating temperature is 390°C-410°C, the heating time is about 60 minutes, and the intensity of the pulse electric field is 100V / mm-300V / mm.
[0028] The present invention adopts a unique pulse electric field heating temperature process: the electric furnace is heated at a heating rate of 2°C-3°C / min, and when the temperature rises to about 96°C, a pulse electrostatic field is loaded onto the sample in the furnace, and the electric field strength is 200V / mm, and the furnace temperature is maintained at this temperature for 30 minutes; after the insulation is completed, the electric furnace is heated to 400°C at a heating rate of 2°C-3°C / min, and the electric field is unloaded after being maintained at 400°C for 60 minutes, and the sample in the furnace is cooled to room temperature along with the furnace.
[0029] Example 1
[0030] Reference Figure 1 The sample of this embodiment uses industrial pure hexahydrate cerium nitrate as raw material. First, hexahydrate cerium nitrate is dissolved in industrial ethanol to prepare an ethanol cerium nitrate solution, and the concentration of cerium nitrate is 10ml / L; the ether solution is stirred at a rate of 60rpm, and the ethanol cerium nitrate solution is atomized and sprayed into the ether solution at a rate of 100ml / min. When the spraying is completed and ethanol is completely dissolved from the ethanol cerium nitrate droplets to form cerium nitrate crystalline particles, 10g / L of phenolic resin is dripped into the ethanol ether solution. After sufficient stirring and dissolution, the ethanol and ether in the solution are evaporated at 90°C using a rotary evaporator, so that the phenolic resin is precipitated and evenly coated on the surface of the cerium nitrate crystalline particles.
[0031] The cerium nitrate crystal particles were dried at 60°C for 12 h, then placed in a corundum tube and sealed. Figure 2In the electric furnace with the temperature field and pulse electric field superimposed, the corundum tube is connected to the pulse power supply. Then the electric furnace is heated at a heating rate of 2℃ / min. When the temperature rises to 96℃, a pulse electrostatic field is applied to the sample in the furnace with an electric field strength of 200V / mm, and the furnace temperature is maintained at this temperature for 30 minutes. After the insulation is completed, the electric furnace is heated to 400℃ at a heating rate of 2℃ / min. After being kept at 400℃ for 60 minutes, the electric field is unloaded and the sample in the furnace is cooled to room temperature along with the furnace.
[0032] During the heating process, when the temperature rises to 96°C, cerium nitrate begins to dehydrate, melt and form molten salt. During the dehydration and decomposition process of cerium nitrate particles, since cerium nitrate is always in a molten state and has ion conductivity, the crystallization process of the particles will change under the induction of an external pulsed electric field. The grain size and grain orientation can be controlled by adjusting the pulsed electric field parameters.
[0033] After heating and crystallization under the induction of a pulse electric field, the sample is taken out of the corundum tube and poured into a corundum crucible. The crucible is then placed in an electric furnace and heated to 1500°C in an air atmosphere and calcined for 60 minutes to remove the solidified resin on the surface of the particles and the carbon produced by its carbonization, thereby improving the crystallinity of the cerium oxide powder particles. Figure 3 This is an electron microscope photo of the cerium oxide powder particles prepared in this example, showing the size of the cerium oxide powder particles and the particle crystal structure inside the particles. It can be seen that the particle size distribution is uniform, the particle diameter is about 1 μm, and the nano-scale particle crystals in the particles are cubic in structure and have a clear directional crystal orientation.
[0034] Compared with the cerium oxide powder prepared by the conventional method, the nano-level fine polishing of this embodiment reduces the consumption of polishing liquid when using the cerium oxide powder prepared by this embodiment, increases the material removal rate by 85.26%, increases the material removal depth by 47.16%, and significantly reduces the pits and scratches on the microscopic surface of the silicon wafer. The line roughness Ra increases by 51.52%, the surface roughness Sa increases by 48.76%, and the nano-level surface accuracy and surface roughness quality of the silicon wafer surface are more than doubled on average.
[0035] Example 2
[0036] Reference Figure 1In this embodiment, the hexahydrate cerium nitrate of embodiment 1 is used as the raw material, and the preparation steps are the same as those of embodiment 1. An ethanol cerium nitrate solution with a cerium nitrate concentration of 20 ml / L is prepared, and the ether solution is stirred at a rate of 60 rpm. At the same time, the ethanol cerium nitrate solution is atomized and sprayed into the ether solution at a rate of 150 ml / min. When ethanol is completely dissolved from the ethanol cerium nitrate droplets to form cerium nitrate crystalline particles, 12 g / L of phenolic resin is dripped into the ethanol ether solution. After sufficient stirring and dissolution, the ethanol and ether in the solution are evaporated at 90°C using a rotary evaporator, so that the phenolic resin is precipitated and evenly coated on the surface of the cerium nitrate crystalline particles. After drying at 60°C for 12 hours, it is loaded into a corundum tube and loaded into an electric furnace. The electric furnace is heated at a heating rate of 3°C / min. When the temperature rises to 96°C, a pulsed electrostatic field is loaded into the furnace with an electric field strength of 250V / mm, and the furnace temperature is maintained for 30 minutes; the electric furnace is then heated to 400°C at a heating rate of 3°C / min, and the electric field is unloaded after being kept at 400°C for 60 minutes. The sample in the furnace is then taken out of the corundum tube and poured into a corundum crucible, which is placed in an electric furnace and heated to 1450°C for 60 minutes for calcination, thereby improving the crystallinity of the cerium oxide powder particles. The particle size distribution of this embodiment is uniform, the particle diameter is about 3μm, and the nano-scale particle crystals have a cubic structure with a clear directional crystal orientation.
[0037] The consumption of polishing liquid during polishing of the cerium oxide powder prepared in this embodiment is significantly reduced, the line roughness Ra is increased by 51.60%, the surface roughness Sa is increased by 48.72%, the material removal rate during polishing is increased by 85.30%, the material removal depth is increased by 47.26%, the pits and scratches on the microscopic surface of the silicon wafer are significantly reduced, and the nano-level surface accuracy and surface roughness quality of the silicon wafer surface are more than doubled on average.
[0038] Example 3
[0039] In this embodiment, cerium nitrate hexahydrate is used as a raw material to prepare an ethanol cerium nitrate solution with a cerium nitrate concentration of 5 ml / L. The ether solution is stirred at a rate of 60 rpm, and the ethanol cerium nitrate solution is atomized and sprayed into the ether solution at a rate of 170 ml / min. When the cerium nitrate crystalline particles are to be generated, 10 g / L of phenolic resin is dripped into the ethanol ether solution, and after sufficient stirring and dissolving, the ethanol and ether in the solution are evaporated at 90 ° C using a rotary evaporator, so that the phenolic resin is precipitated and evenly coated on the surface of the cerium nitrate crystalline particles. After drying at 60 ° C for 12 hours, it is loaded into a corundum tube and loaded into an electric furnace. The electric furnace is heated at a heating rate of 2 ° C / min. When the temperature rises to 96 ° C, a pulsed electrostatic field is loaded into the furnace with an electric field strength of 200 V / mm, and the furnace temperature is maintained for 30 minutes; then the electric furnace is heated to 400 ° C at a heating rate of 2 ° C / min, and the electric field is unloaded after being kept at 400 ° C for 60 minutes, and the sample in the furnace is cooled to room temperature with the furnace. Then the sample was heated to 1500°C in an electric furnace and kept at this temperature for 60 minutes for calcination. The particle size distribution of this embodiment is uniform, the particle diameter is about 2 μm, and has a clear directional crystal orientation.
[0040] After fine polishing of cerium oxide powder, the line roughness Ra of this embodiment is improved by 51.53%, the surface roughness Sa is improved by 48.75%, the material removal rate during polishing is improved by 85.28%, the material removal depth is improved by 47.16%, the microscopic surface roughness of the silicon wafer is greatly improved, and the nano-level surface accuracy and surface roughness quality of the silicon wafer surface are improved by more than double on average.
[0041] Example 4
[0042] Reference Figure 1 In this embodiment, the hexahydrate cerium nitrate of embodiment 1 is also used as a raw material to prepare an ethanol cerium nitrate solution with a cerium nitrate concentration of 15 ml / L, and the ether solution is stirred at a rate of 60 rpm, and the ethanol cerium nitrate solution is atomized and sprayed into the ether solution at a rate of 200 ml / min. After fine polishing of the cerium oxide powder in this embodiment, the line roughness Ra is increased by 51.51%, the surface roughness Sa is increased by 48.72%, the material removal rate during polishing is increased by 85.28%, and the material removal depth is increased by 47.36%. A high-performance cerium oxide powder polishing material with uniform particle size distribution, a particle diameter of about 2 μm, a cubic structure of nano-scale particle crystals in the particles, and obvious directional crystal orientation is prepared.
[0043] The above are only preferred embodiments of the present invention. For ordinary technicians in this technical field, various improvements can be made without departing from the design principles of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.
Claims
1. A method for preparing a cerium oxide powder polishing material, It is characterized in that Using cerium nitrate hexahydrate as raw material, a high-performance cerium oxide powder polishing material is prepared by combining anti-solvent crystallization precipitation method and pulse electric field heating. The process steps are as follows: 1) Preparation of spherical particles of cerium nitrate hexahydrate; dissolving the cerium nitrate hexahydrate in ethanol to prepare an ethanol cerium nitrate solution with a cerium nitrate concentration of 5 ml / L-20 ml / L, atomizing the ethanol cerium nitrate solution into droplets using an atomizer and spraying the droplets into the ether solution, so that the cerium nitrate hexahydrate is completely precipitated in the ether ethanol solution and forms spherical cerium nitrate crystal particles; the volume ratio of ether to ethanol in the ether ethanol solution formed after the cerium nitrate hexahydrate is completely precipitated is 1:1; 2) adding 8 g / L-12 g / L of the phenolic resin to the ether-ethanol solution used to generate the spherical cerium nitrate crystal particles, stirring and dissolving and evaporating the solution, removing the ethanol and ether in the solution, allowing the phenolic resin to precipitate and evenly coat the surface of the spherical cerium nitrate crystal particles, and drying; 3) using pulse electric field heating to decompose the dried spherical cerium nitrate crystal particles to prepare cerium nitrate powder particles; 4) further calcining the cerium nitrate powder particles to remove the carbon coating on the surface of the cerium nitrate powder particles and strengthen the crystal structure thereof, and finally obtaining a nano-scale high-performance cerium oxide powder polishing material.
2. The preparation method according to claim 1, It is characterized in that Use atomizer and The ethanol cerium nitrate solution is atomized into droplets and sprayed into the ether solution at a rate of 100 ml / min-200 ml / min.
3. The preparation method according to claim 1 or 2, It is characterized in that The ether solution was stirred at a rate of 60 rpm.
4. The preparation method according to claim 1, It is characterized in that The evaporation of the phenolic resin is performed at 90°C.
5. The preparation method according to claim 1, It is characterized in that The drying temperature of the spherical cerium nitrate crystal particles is 50° C.-60° C., and the drying time is about 12 hours.
6. The preparation method according to claim 1, It is characterized in that The pulse electric field heating temperature is 390° C.-410° C., the heating time is about 60 minutes, and the intensity of the pulse electric field is 100 V / mm-300 V / mm.
7. The preparation method according to claim 6, It is characterized in that The pulse electric field heating temperature process is: The electric furnace was heated at a heating rate of 2℃-3℃ / min. When the temperature reached about 96℃, a pulse electrostatic field was applied to the sample in the furnace with an electric field strength of 200V / mm. At the same time, the furnace temperature was maintained at this temperature for 30min. After the insulation was completed, the electric furnace was heated to 400℃ at a heating rate of 2℃-3℃ / min. After being maintained at 400℃ for 60min, the electric field was unloaded and the sample in the furnace was cooled to room temperature along with the furnace.
8. The preparation method according to claim 1, It is characterized in that The calcination is to place the cerium nitrate powder particles in a crucible, and then place the crucible in an electric furnace, heat it to 1400° C.-1500° C. and keep it warm for 60 minutes.
9. The preparation method according to claim 1, It is characterized in that The nanometer-level high-performance cerium oxide powder polishing material is a nanometer-level particle crystal with a diameter of 1 μm to 3 μm and a particle size in a cubic structure, and has an obvious directional crystal orientation.