Method for preparing dendritic cuprous oxide under normal pressure

By using reducing sugar and complexing agent under normal pressure, the problems of complexing dendritic copper oxide preparation equipment in the prior art are solved, and efficient and low-cost dendritic copper oxide preparation are achieved. In various materials applications.

CN118929732APending Publication Date: 2024-11-12YOUYAN POWDER NEW MATERIALS (HEFEI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411293170.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the preparation methods of dendritic copper oxide are mostly electrodeposition methods, with complex equipment and low yields, or chemical reduction methods but require high pressure and high temperature, which limits industrial production.

Method used

The dendritic copper oxide was prepared by using the method under normal pressure, reducing sugar was used as the copper ion reducing agent and adding a complexing agent. The operation was simple, the cost was low and the yield was high.

Benefits of technology

It has achieved efficient preparation of dendritic copper oxide under normal pressure, with a large surface area, suitable for catalysts, gas sensors, antibacterial materials and other fields, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929732A_ABST
    Figure CN118929732A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing dendritic cuprous oxide under normal pressure, and belongs to the technical field of cuprous oxide, the preparation method comprises the following steps: adding a complexing agent into a NaOH solution for stirring, dropwise adding a copper salt solution into the continuously stirred NaOH solution at room temperature, stirring for 5-30 minutes, then adding into a reducing sugar solution, and heating for reaction; and after the reaction is finished, cooling, washing, filtering and drying to obtain the dendritic cuprous oxide. According to the method, reducing sugar is adopted as a copper ion reducing agent, only reaction is needed under normal pressure after a complexing agent is added, and the prepared dendritic cuprous oxide has a large surface area and can be applied to the fields of catalysts, gas sensors, antibacterial materials, photoelectric materials and the like; the preparation method is simple, equipment is simple, stability is good, yield is high, and industrial production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cuprous oxide, and in particular relates to a method for preparing dendritic cuprous oxide under normal pressure. Background Art

[0002] Cuprous oxide is a new type of P-type semiconductor material with active hole-electron pairs and good catalytic activity. It has a wide range of applications in many fields due to its unique properties. In addition to its good catalytic activity, cuprous oxide also has strong adsorption properties, bactericidal activity, photoelectric conversion and other characteristics. It can be used in catalysts, gas sensors, antibacterial materials, photoelectric materials and other fields.

[0003] Cuprous oxide with a more complex morphology, namely dendritic cuprous oxide, can not only increase the specific surface area of ​​the material, enhance performance, improve stability and optimize reaction or sensing characteristics, but also provide more active sites, while improving the electronic structure and optical properties of the material, thereby improving its application in downstream materials.

[0004] Most of the dendritic cuprous oxide reported in the literature is prepared by electrodeposition, which has the problems of complex equipment, serious agglomeration, and low yield. There are also patents reporting the preparation of dendritic cuprous oxide by chemical reduction, but the raw materials used are toxic, high pressure is required, the reaction temperature is high, and the reaction time is long, which is not conducive to industrial production. Summary of the invention

[0005] The present invention aims to provide a method for preparing dendritic cuprous oxide under normal pressure, which has simple experimental conditions and operation, good repeatability, low cost and high yield. The method uses reducing sugar as a copper ion reducing agent, adds a complexing agent, and slowly heats the reaction to prepare dendritic cuprous oxide.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing dendritic cuprous oxide under normal pressure comprises the following steps:

[0008] The complexing agent is added into the NaOH solution and stirred. The copper salt solution is added dropwise into the constantly stirred NaOH solution at room temperature and stirred for 5-30 minutes. Then, the solution is added into the reducing sugar solution and heated for reaction. After the reaction is completed, the solution is cooled, washed, filtered and dried to obtain the dendritic cuprous oxide.

[0009] As a further embodiment of the present invention, the dosage ratio of the complexing agent, the NaOH solution, the copper salt solution and the reducing sugar solution is 0.025-0.05 mol: 50 mL: 50 mL: 50-200 mL.

[0010] As a further solution of the present invention, the concentration of the NaOH solution is 2.5 mol / L.

[0011] As a further embodiment of the present invention, the concentration of the copper salt solution is 0.5-1.0 mol / L.

[0012] As a further embodiment of the present invention, the concentration of the reducing sugar solution is 0.5-2 mol / L.

[0013] As a further embodiment of the present invention, the complexing agent is one of potassium sodium tartrate and sodium tartrate.

[0014] As a further embodiment of the present invention, the copper salt is one of copper sulfate pentahydrate and copper acetate.

[0015] As a further embodiment of the present invention, the reducing sugar is one of glucose, maltose, fructose, galactose and lactose.

[0016] As a further solution of the present invention, the temperature is heated to 60-70° C. and the reaction time is 0.5-2 h.

[0017] Beneficial effects of the present invention:

[0018] The invention discloses a method for preparing dendritic cuprous oxide under normal pressure, which adopts reducing sugar as a copper ion reducing agent and adds a complexing agent to influence the preferential growth of copper in the copper ion reduction process. The reaction is carried out under normal pressure, has a short reaction time, is simple to operate, has low requirements on equipment, has good stability, high yield and is convenient for industrial production.

[0019] The dendritic cuprous oxide prepared by the present invention has a large surface area and can be applied to the fields of catalysts, gas sensors, antibacterial materials, photoelectric materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described below in conjunction with the accompanying drawings.

[0021] Figure 1 is a SEM image of the dendritic cuprous oxide obtained in Example 1 of the present invention;

[0022] Figure 2 is a SEM image of the dendritic cuprous oxide obtained in Example 2 of the present invention;

[0023] Figure 3 is a SEM image of the dendritic cuprous oxide obtained in Example 3 of the present invention;

[0024] Figure 4 is a SEM image of the dendritic cuprous oxide obtained in Example 4 of the present invention;

[0025] Figure 5It is the XRD diagram of the product obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] This embodiment provides a method for preparing dendritic cuprous oxide under normal pressure, comprising the following steps:

[0029] Prepare 50 mL of 1.0 mol / L copper sulfate pentahydrate solution, 50 mL of 2.5 mol / L NaOH solution, and 100 mL of 1.0 mol / L glucose solution;

[0030] 0.05 mol of potassium sodium tartrate was added to 50 mL of 2.5 mol / L NaOH solution and stirred. 50 mL of 1.0 mol / L copper sulfate pentahydrate solution was added dropwise to the constantly stirred NaOH solution at room temperature and stirred for 30 min. Then, 100 mL of 1.0 mol / L glucose solution was added dropwise and the mixture was placed in a water bath and slowly heated to 60°C for reaction for 1 h. After the reaction was completed, the heating system was turned off and the temperature was slowly lowered. Then, the mixture was washed and filtered with deionized water and anhydrous ethanol for 5 times respectively and dried in a vacuum drying oven at 80°C to obtain dendritic cuprous oxide.

[0031] The morphology of the product was observed by scanning electron microscopy (SEM). The SEM morphology of the obtained dendrite-like cuprous oxide is as follows: Figure 1 As shown; the material structure of the product was characterized by X-ray diffractometer (XRD), and the XRD spectrum of the obtained dendrite-state cuprous oxide was as follows Figure 5 shown.

[0032] Example 2

[0033] This embodiment provides a method for preparing dendritic cuprous oxide under normal pressure, comprising the following steps:

[0034] Prepare 50 mL of 1.0 mol / L copper sulfate pentahydrate solution, 50 mL of 2.5 mol / L NaOH solution, and 200 mL of 0.5 mol / L maltose solution;

[0035] 0.05 mol of potassium sodium tartrate was added to 50 mL of 2.5 mol / L NaOH solution and stirred. 50 mL of 1.0 mol / L copper sulfate pentahydrate solution was added dropwise to the constantly stirred NaOH solution at room temperature and stirred for 30 min. Then, 200 mL of 0.5 mol / L maltose solution was added dropwise, and then the mixture was slowly heated to 70°C in a water bath for reaction for 1 h. After the reaction was completed, the heating system was turned off and the temperature was slowly lowered. Then, the mixture was washed and filtered with deionized water and anhydrous ethanol for 5 times, respectively, and dried in a vacuum drying oven at 80°C to obtain dendritic cuprous oxide.

[0036] The morphology of the product was observed by scanning electron microscopy (SEM). The SEM morphology of the obtained dendrite-like cuprous oxide is as follows: Figure 2 shown.

[0037] Example 3

[0038] This embodiment provides a method for preparing dendritic cuprous oxide under normal pressure, comprising the following steps:

[0039] Prepare 50 mL of 0.5 mol / L copper acetate solution, 50 mL of 2.5 mol / L NaOH solution, and 100 mL of 0.5 mol / L glucose solution;

[0040] 0.025 mol of sodium tartrate was added to 50 mL of 2.5 mol / L NaOH solution and stirred. 50 mL of 0.5 mol / L copper acetate solution was added dropwise to the constantly stirred NaOH solution at room temperature and stirred for 30 min. Then, 100 mL of 0.5 mol / L glucose solution was added dropwise. Then, the mixture was slowly heated to 70°C in a water bath and reacted for 1 h. After the reaction was completed, the heating system was turned off and the temperature was slowly lowered. Then, the mixture was washed and filtered with deionized water and anhydrous ethanol for 5 times respectively, and dried in a vacuum drying oven at 80°C to obtain dendritic cuprous oxide.

[0041] The morphology of the product was observed by scanning electron microscopy (SEM). The SEM morphology of the obtained dendrite-like cuprous oxide is as follows: Figure 3 shown.

[0042] Example 4

[0043] This embodiment provides a method for preparing dendritic cuprous oxide under normal pressure, comprising the following steps:

[0044] Prepare 50 mL of 1.0 mol / L copper acetate solution, 50 mL of 3.0 mol / L NaOH solution, and 50 mL of 2.0 mol / L maltose solution;

[0045] 0.05 mol of sodium tartrate was added to 50 mL of 3.0 mol / L NaOH solution and stirred. 50 mL of 1.0 mol / L copper acetate solution was added dropwise to the constantly stirred NaOH solution at room temperature and stirred for 30 min. Then, 50 mL of 2.0 mol / L maltose solution was added dropwise. Then, the mixture was slowly heated to 60°C in a water bath and reacted for 1 h. After the reaction, the heating system was turned off and the temperature was slowly lowered. Then, the mixture was washed and filtered with deionized water and anhydrous ethanol for 5 times, respectively, and dried in a vacuum drying oven at 80°C to obtain dendritic cuprous oxide.

[0046] The morphology of the product was observed by scanning electron microscopy (SEM). The SEM morphology of the obtained dendrite-like cuprous oxide is as follows: Figure 4 shown.

[0047] Depend on Figure 1 It can be seen that the dendritic cuprous oxide trunk grows along the

[100] ,

[010] , and

[001] crystal directions, and the branches are perpendicular to the trunk. Upon closer observation, it can be found that the branch structure is composed of multiple crystal planes of different indices, and the side branches on the same side are arranged parallel to each other, and the trunk and branches form a three-dimensional structure.

[0048] Depend on Figure 5 It can be seen that the XRD pattern of the dendritic cuprous oxide prepared in Example 1 is consistent with the diffraction pattern of the card No. JCPDS 05-0667 in the X-ray diffraction database, indicating that the products obtained in the experiment are all Cu2O crystals, the crystals belong to the isometric crystal system, the space group is (224), the unit cell parameters are a0=b0=c0=0.4296nm, α=β=γ=90°.

[0049] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing dendritic cuprous oxide under normal pressure, characterized in that: The following steps are involved: The complexing agent is added into the NaOH solution and stirred. The copper salt solution is added dropwise into the constantly stirred NaOH solution at room temperature and stirred for 5-30 minutes. Then, the solution is added into the reducing sugar solution and heated for reaction. After the reaction is completed, the solution is cooled, washed, filtered and dried to obtain the dendritic cuprous oxide.

2. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The dosage ratio of the complexing agent, the NaOH solution, the copper salt solution and the reducing sugar solution is 0.025-0.05 mol: 50 mL: 50 mL: 50-200 mL.

3. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The concentration of the NaOH solution is 2.5 mol / L.

4. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The concentration of the copper salt solution is 0.5-1.0 mol / L.

5. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The concentration of the reducing sugar solution is 0.5-2 mol / L.

6. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The complexing agent is one of potassium sodium tartrate and sodium tartrate.

7. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The copper salt is one of copper sulfate pentahydrate and copper acetate.

8. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: The reducing sugar is one of glucose, maltose, fructose, galactose and lactose.

9. The method for preparing dendritic cuprous oxide under normal pressure according to claim 1, characterized in that: Heat to 60-70°C, reaction time is 0.5-2h.