Clustered zinc oxide and preparation method thereof

By preparing clustered zinc oxide with high specific surface area, the problem of insufficient dielectric performance of zinc oxide in the prior art is solved, and the performance improvement in dielectric materials is achieved.

CN118929734APending Publication Date: 2024-11-12UNIV OF ELECTRONICS SCI & TECH OF CHINA +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411188419.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing nano zinc oxide preparation methods are difficult to obtain clustered zinc oxide with high specific surface area, and the dielectric performance is insufficient in the application of dielectric materials.

Method used

Using a step that includes polythiophene preparation, reaction solution configuration and solvothermal reaction, by stirring ferric chloride and thiophene at room temperature, followed by addition of soluble zinc salt and hydroxide, mechanical stirring and solvothermal reaction, and finally Separation and drying under low temperature conditions to obtain clustered zinc oxide with high specific surface area.

Benefits of technology

High purity preparation of clustered zinc oxide is achieved, with a high specific surface area, and significantly improves dielectric properties in dielectric materials such as polyvinylidene fluoride.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929734A_ABST
    Figure CN118929734A_ABST
Patent Text Reader

Abstract

The invention provides clustered zinc oxide and a preparation method thereof. The preparation method comprises the following steps: step 1, preparing polythiophene; 2, preparing a water reaction solution; step 3, solvothermal reaction; and 4, separating, washing and drying the product. The polythiophene is reticular, so that the purity of the clustered zinc oxide can be indirectly improved. The zinc oxide material is novel in structure, has a relatively high specific surface area, and can effectively improve the dielectric property when being doped in dielectric materials such as polyvinylidene fluoride (PVDF) and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal-inorganic composite materials, and particularly relates to clustered zinc oxide and a preparation method thereof. Background Art

[0002] Zinc oxide (ZnO), as a new type of inorganic material, has long been widely used in rubber, dyes, inks, coatings, glass, ceramics, optoelectronics and other fields. Compared with traditional ZnO used as an inorganic chemical material, nano ZnO has a dramatically increased specific surface area, and its surface molecular arrangement, electronic structure and crystal structure have undergone significant changes. It has surface effects, small size effects, quantum size effects, macroscopic quantum tunneling effects, etc. It has special properties and uses in magnetism, light, electricity, catalysis and other aspects that traditional ZnO cannot match, so it has received widespread attention in recent years.

[0003] Nano zinc oxide was first produced by gas phase synthesis in the 1980s. Subsequently, the preparation of nano zinc oxide has been further studied in the world, and there are currently a variety of preparation methods. The morphology of nano zinc oxide obtained by different preparation processes can be different, usually in the form of rods, flakes, spheres, etc., and its properties are also different.

[0004] Clustered nano zinc oxide is a nanomaterial with a specific morphology. Its structure is similar to flowers or clusters. This special morphology can provide a large specific surface area and unique physical and chemical properties. In the field of photocatalysis, clustered nano zinc oxide has attracted much attention due to its high specific surface area and ability to delay the recombination of electrons and holes. These properties help to improve photocatalytic activity. In practical applications, clustered nano zinc oxide can not only be used for photocatalytic degradation of organic pollutants, but also as a functional filler for sensors, optoelectronic materials, coatings, etc. Due to its biocompatibility, clustered nano zinc oxide also shows potential application value in the biomedical field. Clustered nano zinc oxide can be prepared by various methods, including hydrothermal method, chemical precipitation method, sol-gel method, etc. These methods can regulate the morphology, size and crystal structure of the material, thereby affecting its photocatalytic performance. For example, the nano zinc oxide array synthesized in situ by hydrothermal method can achieve layered absorption of sunlight, reduce heat energy loss, and improve light energy utilization. Summary of the invention

[0005] The invention mainly discloses a novel clustered zinc oxide with a high specific surface area, which can effectively improve the dielectric properties when doped in dielectric materials such as polyvinylidene fluoride (PVDF).

[0006] In order to obtain the above-mentioned clustered zinc oxide, the technical solution adopted by the present invention is:

[0007] A method for preparing clustered zinc oxide, characterized by comprising the following steps:

[0008] Step 1: Preparation of polythiophene

[0009] (1.1) At room temperature, weigh ferric chloride and add it to chloroform in a ratio of 0.12 mol to 0.15 mol:100 ml of chloroform. Stir for 1 to 2 hours to obtain a ferric chloride solution.

[0010] (1.2) Weigh thiophene and add it to chloroform in a ratio of 0.02 mol to 0.05 mol:100 ml of chloroform. Ultrasonic dispersion is performed for 10 to 30 minutes to obtain a thiophene dispersion.

[0011] (1.3) dispersing the thiophene dispersion dropwise into a ferric chloride solution, wherein the molar ratio of ferric chloride to thiophene is 3:1 to 4:1, to obtain a solution;

[0012] (1.4) The solution obtained in (1.3) was stirred at 0-5°C for 10-12 hours at a stirring rate of 500-800 rpm. After the reaction, the solvent was evaporated at 30°C to obtain a reddish brown powder;

[0013] (1.5) The obtained reddish brown powder was stirred in a 1 mol / L HCl solution for 12 hours and washed several times, and the product was dried in an oven at 40 to 60° C. to obtain polythiophene;

[0014] Step 2: Preparation of reaction solution

[0015] (2.1) At room temperature, weigh a soluble zinc salt and a hydroxide in a molar ratio of 1:1 to 1:4, add them to deionized water, and stir mechanically for 20 to 30 minutes;

[0016] (2.2) adding a mixed solvent of ethylenediamine and ethanolamine in a volume ratio of 1:3 to 3:1 to the solution;

[0017] (2.3) mechanically stirring the solution for 20 to 40 minutes to obtain a clear reaction solution, wherein the ratio of the total amount of soluble zinc salt and hydroxide to deionized water is 0.07 g to 0.5 g: 1 ml, and the volume ratio of the added mixed solvent to deionized water is 1:6 to 1:1;

[0018] (2.4) adding the polythiophene synthesized in step 1 to the solution, wherein the mass ratio of the added polythiophene to the soluble zinc salt is 1:15 to 1:10, and mechanically stirring for 30 to 60 minutes;

[0019] Step 3: Solvothermal reaction

[0020] (3.1) Place the above reaction solution in a reactor and perform a solvent thermal reaction at a temperature of 90 to 130°C for 12 to 24 hours, and then cool naturally to room temperature;

[0021] Step 4: Product separation, washing and drying

[0022] (4.1) The product is centrifuged at a speed of 6000-8000 rpm for 10-20 minutes, washed with deionized water and anhydrous ethanol for 1-3 times, respectively, and dried at 40-60°C for 5-8 hours to obtain clustered zinc oxide.

[0023] As a preferred embodiment, the molar ratio of ferric chloride to thiophene in the step (1.3) is 3:1.

[0024] As a preferred embodiment, the soluble zinc salt in step (2.1) is selected from zinc acetate, zinc nitrate, zinc chloride or zinc sulfate.

[0025] As a preferred embodiment, the hydroxide in step (2.1) is selected from potassium hydroxide, sodium hydroxide, lithium hydroxide or ammonia water.

[0026] As a preferred embodiment, the volume ratio of ethylenediamine to ethanolamine in step (2.2) is 1:1.

[0027] The second object of the present invention is to provide a clustered zinc oxide obtained by the preparation method.

[0028] As a preferred method, the preparation of polythiophene in step 1 can be carried out by electrochemical polymerization.

[0029] The beneficial effects of the present invention are:

[0030] (1) The preparation method of the present invention is simple, the temperature is low, and it is easy to control;

[0031] (2) The clustered zinc oxide prepared by the present invention has high purity and is not easy to generate impurities in the organic phase.

[0032] (3) The zinc oxide material in the present invention has a novel structure and a high specific surface area. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a SEM image of the network polythiophene prepared in step 1 of the present invention.

[0034] Figure 2 It is a SEM picture of clustered zinc oxide prepared by the present invention.

[0035] Figure 3 It is the XRD spectrum of the clustered zinc oxide prepared by the present invention. DETAILED DESCRIPTION

[0036] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0037] Example 1

[0038] The embodiment provides a method for preparing clustered zinc oxide, comprising the following steps:

[0039] Step 1: Preparation of polythiophene

[0040] (1.1) At room temperature, weigh ferric chloride and add it to chloroform in a ratio of 0.12 mol:100 ml of chloroform. Stir for 1 hour to obtain a ferric chloride solution.

[0041] (1.2) Weigh thiophene and add it to chloroform at a ratio of 0.02 mol:100 ml of chloroform. Ultrasonic dispersion is performed for 10 minutes to obtain a thiophene dispersion.

[0042] (1.3) dispersing the thiophene dispersion dropwise into a ferric chloride solution, wherein the molar ratio of ferric chloride to thiophene is 3:1, to obtain a solution;

[0043] (1.4) The solution obtained in (1.3) was stirred at 0°C for 10 hours at a stirring rate of 500 rpm. After the reaction was completed, the solvent was evaporated at 30°C to obtain a reddish brown powder;

[0044] (1.5) The obtained reddish brown powder was stirred in a 1 mol / L HCl solution for 12 hours and washed several times, and the product was dried in an oven at 4°C to obtain polythiophene;

[0045] Step 2: Preparation of reaction solution

[0046] (2.1) At room temperature, weigh a soluble zinc salt and a hydroxide in a molar ratio of 1:1, add them to deionized water, and stir mechanically for 20 minutes; the soluble zinc salt is selected from zinc nitrate, and the hydroxide is selected from sodium hydroxide.

[0047] (2.2) adding a mixed solvent of ethylenediamine and ethanolamine in a volume ratio of 1:3 to the solution;

[0048] (2.3) The solution was mechanically stirred for 20 minutes to obtain a clear reaction solution, wherein the ratio of the total amount of soluble zinc salt and hydroxide to deionized water was 0.07 g:1 ml, and the volume ratio of the added mixed solvent to deionized water was 1:6;

[0049] (2.4) adding the polythiophene synthesized in step 1 to the solution, wherein the mass ratio of the added polythiophene to the soluble zinc salt is 1:15, and mechanically stirring for 30 minutes;

[0050] Step 3: Solvothermal reaction

[0051] (3.1) The above reaction solution was placed in a reactor for solvothermal reaction at 90°C for 12 hours and then cooled naturally to room temperature;

[0052] Step 4: Product separation, washing and drying

[0053] (4.1) The product was centrifuged at a speed of 6000 rpm for 10 minutes, washed with deionized water and anhydrous ethanol for 1 to 3 times, respectively, and dried at 40°C for 5 hours to obtain clustered zinc oxide.

[0054] The preparation method obtains clustered zinc oxide. The SEM image of clustered zinc oxide is as follows Figure 2 As shown, the XRD pattern of clustered zinc oxide is as follows Figure 3 shown.

[0055] Example 2

[0056] The embodiment provides a method for preparing clustered zinc oxide, comprising the following steps:

[0057] Step 1: Preparation of polythiophene

[0058] (1.1) At room temperature, weigh ferric chloride and add it to chloroform in a ratio of 0.15 mol to 100 ml of chloroform. Stir for 2 hours to obtain a ferric chloride solution.

[0059] (1.2) Weigh thiophene and add it to chloroform at a ratio of 0.05 mol:100 ml of thiophene and disperse it by ultrasonic for 30 minutes to obtain a thiophene dispersion;

[0060] (1.3) dispersing the thiophene dispersion dropwise into a ferric chloride solution, wherein the molar ratio of ferric chloride to thiophene is 4:1, to obtain a solution;

[0061] (1.4) The solution obtained in (1.3) was stirred at 5°C for 12 hours at a stirring rate of 800 rpm. After the reaction was completed, the solvent was evaporated at 30°C to obtain a reddish brown powder;

[0062] (1.5) The obtained reddish brown powder was stirred in a 1 mol / L HCl solution for 12 hours and washed several times, and the product was dried in an oven at 60° C. to obtain polythiophene;

[0063] Step 2: Preparation of reaction solution

[0064] (2.1) At room temperature, weigh a soluble zinc salt and a hydroxide in a molar ratio of 1:4, add them to deionized water, and stir mechanically for 30 minutes; the soluble zinc salt is selected from zinc chloride and the hydroxide is selected from lithium hydroxide.

[0065] (2.2) adding a mixed solvent of ethylenediamine and ethanolamine in a volume ratio of 3:1 to the solution;

[0066] (2.3) The solution was mechanically stirred for 40 minutes to obtain a clear reaction solution, wherein the ratio of the total amount of soluble zinc salt and hydroxide to deionized water was 0.5 g:1 ml, and the volume ratio of the added mixed solvent to deionized water was 1:1;

[0067] (2.4) adding the polythiophene synthesized in step 1 to the solution, wherein the mass ratio of the added polythiophene to the soluble zinc salt is 1:10, and mechanically stirring for 60 minutes;

[0068] Step 3: Solvothermal reaction

[0069] (3.1) The above reaction solution was placed in a reaction vessel for solvothermal reaction at a temperature of 130°C for 12 to 24 hours, and then naturally cooled to room temperature;

[0070] Step 4: Product separation, washing and drying

[0071] (4.1) The product was centrifuged at a speed of 8000 rpm for 20 minutes, washed with deionized water and anhydrous ethanol three times respectively, and dried at 60°C for 8 hours to obtain clustered zinc oxide.

[0072] The preparation method obtains clustered zinc oxide. The SEM image of clustered zinc oxide is as follows Figure 2 As shown, the XRD pattern of clustered zinc oxide is as follows Figure 3 shown.

[0073] Example 3

[0074] The embodiment provides a method for preparing clustered zinc oxide, comprising the following steps:

[0075] Step 1: Preparation of polythiophene

[0076] (1.1) At room temperature, weigh ferric chloride and add it to chloroform in a ratio of 0.14 mol to 100 ml of chloroform. Stir for 1.5 hours to obtain a ferric chloride solution.

[0077] (1.2) Weigh thiophene and add it to chloroform at a ratio of 0.03 mol:100 ml of chloroform. Ultrasonic dispersion is performed for 20 minutes to obtain a thiophene dispersion.

[0078] (1.3) dispersing the thiophene dispersion dropwise into a ferric chloride solution, wherein the molar ratio of ferric chloride to thiophene is 3.51, to obtain a solution;

[0079] (1.4) The solution obtained in (1.3) was stirred at 3°C ​​for 11 hours at a stirring rate of 600 rpm. After the reaction was completed, the solvent was evaporated at 30°C to obtain a reddish brown powder;

[0080] (1.5) The obtained reddish brown powder was stirred in a 1 mol / L HCl solution for 12 hours and washed several times. The product was dried in an oven at 50°C to obtain a network of polythiophene, such as Figure 1 As shown;

[0081] Step 2: Preparation of reaction solution

[0082] (2.1) At room temperature, weigh a soluble zinc salt and a hydroxide in a molar ratio of 1:3, add them to deionized water, and stir mechanically for 25 minutes; the soluble zinc salt is selected from zinc sulfate, and the hydroxide is selected from ammonia water.

[0083] (2.2) adding a mixed solvent of ethylenediamine and ethanolamine in a volume ratio of 1:1 to the solution;

[0084] (2.3) The solution was mechanically stirred for 30 minutes to obtain a clear reaction solution, wherein the ratio of the total amount of soluble zinc salt and hydroxide to deionized water was 0.2 g:1 ml, and the volume ratio of the added mixed solvent to deionized water was 2:1;

[0085] (2.4) adding the polythiophene synthesized in step 1 to the solution, wherein the mass ratio of the added polythiophene to the soluble zinc salt is 1:12, and mechanically stirring for 40 minutes;

[0086] Step 3: Solvothermal reaction

[0087] (3.1) The above reaction solution was placed in a reactor for solvothermal reaction at a temperature of 1000°C for 16 hours, and then naturally cooled to room temperature;

[0088] Step 4: Product separation, washing and drying

[0089] (4.1) The product was centrifuged at a speed of 7000 rpm for 15 minutes, washed twice with deionized water and anhydrous ethanol respectively, and dried at 50°C for 6 hours to obtain clustered zinc oxide.

[0090] The preparation method obtains clustered zinc oxide. The SEM image of clustered zinc oxide is as follows Figure 2 As shown, the XRD pattern of clustered zinc oxide is as follows Figure 3 shown.

[0091] Example 4

[0092] The embodiment provides a method for preparing clustered zinc oxide, comprising the following steps:

[0093] Step 1: Preparation of polythiophene

[0094] (1.1) At room temperature, weigh 9.75 g of ferric chloride and add it to 50 ml of chloroform, and stir for 1 hour to obtain a ferric chloride solution;

[0095] (1.2) Weigh 1.68 g of thiophene and add it to 50 ml of chloroform, and disperse it by ultrasonic for 30 minutes to obtain a thiophene dispersion;

[0096] (1.3) dispersing the thiophene dispersion dropwise into the ferric chloride solution to obtain a solution;

[0097] (1.4) The solution obtained in (1.3) was stirred at 0°C and 500 rpm for 12 hours. After the reaction was completed, the solvent was evaporated at 30°C to obtain a reddish brown powder;

[0098] (1.5) The obtained product was stirred in a 1 mol / L HCl solution for 12 hours and washed several times, and the product was dried in an oven at 50° C. to obtain polythiophene;

[0099] Step 2: Preparation of reaction solution

[0100] (2.1) At room temperature, weigh 1 g zinc acetate and 1 g potassium hydroxide, add them to 15 ml deionized water, and stir mechanically for 20 minutes;

[0101] (2.2) Add 15 ml of a mixed solvent of ethylenediamine and 15 ml of ethanolamine to the solution;

[0102] (2.3) Mechanically stirring for 40 minutes to obtain a clear reaction solution;

[0103] (2.4) adding 0.1 g of polythiophene synthesized in step 1 and mechanically stirring for 60 minutes;

[0104] Step 3: Solvothermal reaction

[0105] (3.1) The above reaction solution was placed in a reactor for solvothermal reaction at 110°C for 12 h and then cooled naturally to room temperature;

[0106] Step 4: Product, separation, washing, drying

[0107] (4.1) The product was centrifuged at 6000 rpm for 15 minutes, washed three times with deionized water and anhydrous ethanol respectively, and dried at 60°C for 6 hours to obtain clustered zinc oxide.

[0108] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing clustered zinc oxide, Features The steps include: Step 1: Preparation of polythiophene (1.1) At room temperature, weigh ferric chloride and add it to chloroform in a ratio of 0.12 mol to 0.15 mol:100 ml of chloroform. Stir for 1 to 2 hours to obtain a ferric chloride solution. (1.2) Weigh thiophene and add it to chloroform in a ratio of 0.02 mol to 0.05 mol:100 ml of chloroform. Ultrasonic dispersion is performed for 10 to 30 minutes to obtain a thiophene dispersion. (1.3) dispersing the thiophene dispersion dropwise into a ferric chloride solution, wherein the molar ratio of ferric chloride to thiophene is 3:1 to 4:1, to obtain a solution; (1.4) The solution obtained in (1.3) was stirred at 0-5°C for 10-12 hours at a stirring rate of 500-800 rpm. After the reaction, the solvent was evaporated at 30°C to obtain a reddish brown powder; (1.5) The obtained reddish brown powder was stirred in a 1 mol / L HCl solution for 12 hours and washed several times, and the product was dried in an oven at 40 to 60° C. to obtain polythiophene; Step 2: Preparation of reaction solution (2.1) At room temperature, weigh a soluble zinc salt and a hydroxide in a molar ratio of 1:1 to 1:4, add them to deionized water, and mechanically stir for 20 to 30 minutes; (2.2) adding a mixed solvent of ethylenediamine and ethanolamine in a volume ratio of 1:3 to 3:1 to the solution; (2.3) mechanically stirring the solution for 20 to 40 minutes to obtain a clear reaction solution, wherein the ratio of the total amount of soluble zinc salt and hydroxide to deionized water is 0.07 g to 0.5 g: 1 ml, and the volume ratio of the added mixed solvent to deionized water is 1:6 to 1:1; (2.4) adding the polythiophene synthesized in step 1 to the solution, wherein the mass ratio of the added polythiophene to the soluble zinc salt is 1:15 to 1:10, and mechanically stirring for 30 to 60 minutes; Step 3: Solvothermal reaction (3.1) Place the above reaction solution in a reaction kettle and perform a solvent thermal reaction at a temperature of 90 to 130° C. for 12 to 24 hours, and then cool naturally to room temperature; Step 4: Product separation, washing and drying (4.1) The product is centrifuged at a speed of 6000-8000 rpm for 10-20 minutes, washed with deionized water and anhydrous ethanol for 1-3 times, respectively, and dried at 40-60° C. for 5-8 hours to obtain clustered zinc oxide.

2. A method for preparing clustered zinc oxide according to claim 1, Features: In the step (1.3), the molar ratio of ferric chloride to thiophene is 3:

1.

3. A method for preparing clustered zinc oxide according to claim 1, Features: The soluble zinc salt in step (2.1) is selected from zinc acetate, zinc nitrate, zinc chloride or zinc sulfate.

4. A method for preparing clustered zinc oxide according to claim 1, Features: In the step (2.1), the hydroxide is selected from potassium hydroxide, sodium hydroxide, lithium hydroxide or ammonia water.

5. A method for preparing clustered zinc oxide according to claim 1, Features: In the step (2.2), the volume ratio of ethylenediamine to ethanolamine is 1:

1.

6. Clustered zinc oxide obtained by the preparation method according to any one of claims 1 to 5.