High-purity titanium dioxide and preparation method thereof

Through the methods of pulverization, acidolysis and hydrothermal reaction, combined with surfactant and modified complexing agent, the problems of low titanium concentration and high impurities in the prior art are solved, the purity and recovery rate of titanium dioxide are improved, and the environment is reduced. Pollution risk is applicable to multiple industries.

CN118929746AActive Publication Date: 2024-11-12HUBEI ZHANPENG ELECTRONIC MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411065400.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

When preparing titanium dioxide from titanium-containing blast furnace slag, the titanium concentration is relatively low and the impurity content is high, resulting in long production processes, large energy consumption, and low titanium recovery rate, making it difficult to achieve industrial application.

Method used

By using the methods of crushing, acid decomposition, hydrothermal reaction and calcination, the impurities are removed by adding surfactant and modification complexing agent during the acid decomposition process, the purity and recovery of titanium are improved, the amount of acid is reduced, and the environment is reduced. Pollution risk.

Benefits of technology

Effectively remove impurities in titanium-containing blast furnace slag, improve the product quality of titanium dioxide, reduce the use of acid, and reduce the risk of environmental pollution. It is suitable for many industries, such as coatings, plastics, papermaking, etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929746A_ABST
    Figure CN118929746A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: crushing, grinding and sieving titanium-containing blast furnace slag, mixing the titanium-containing blast furnace slag with a sulfuric acid solution, adding a modified complexing agent and a surfactant, carrying out a heating reaction to obtain acidolysis slag, adding the acidolysis slag into deionized water, carrying out stirring mixing to obtain an impurity-containing titanyl sulfate solution, adding the impurity-containing titanyl sulfate solution into a reaction kettle, carrying out stirring reaction for 2-3 hours, and carrying out vacuum drying to obtain the high-purity titanium dioxide. The preparation method comprises the following steps: taking titanium dioxide as a raw material, performing sealed reaction to obtain hydrothermal metatitanic acid, mixing the hydrothermal metatitanic acid with a NaOH solution to prepare slurry, adjusting the pH value, stirring at normal temperature, filtering, washing and drying a product to obtain desulfurized metatitanic acid, roasting and cooling to obtain the high-purity titanium dioxide, according to the method provided by the invention, impurities in the titanium-containing blast furnace slag can be effectively removed, the product quality of the prepared titanium dioxide is improved, the use amount of acid is reduced, and the risk of environmental pollution is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium dioxide, and in particular to high-purity titanium dioxide and a preparation method thereof. Background Art

[0002] Titanium-bearing furnace slag (TBFS) is a byproduct of blast furnace smelting of vanadium-titanium magnetite and is a valuable titanium resource that needs to be developed. During blast furnace smelting, unreduced oxides of titanium, silicon, calcium, magnesium, aluminum, etc., melt together with vanadium-containing molten iron, titanium carbide, and titanium nitride at 1385-1440°C and crystallize and solidify at 1000-1200°C to form TBFS.

[0003] The main mineral components of TBFS are perovskite and tantalum diopside, and contain a small amount of titanium-rich diopside, magnesium-aluminum spinel, titanium carbide and titanium nitride. Titanium resources are dispersed in a variety of mineral phases. The titanium-containing mineral grains are small (about 10μm), chaotically distributed, and intergrowth. The traditional mineral processing and smelting technology cannot separate the titanium-containing components from the slag phase. Only a very small part is used to prepare low-end building materials (such as slag cement, sanitary porcelain panels and alkali-resistant mineral wool, etc.). A large amount of titanium-containing blast furnace slag is idle. The total accumulation has exceeded 80 million tons and is increasing at a rate of more than 3.8 million tons per year. The sustainable development of the vanadium-titanium industry faces great environmental pressure. It is urgent to solve the bottleneck of TBFS utilization through technological innovation and promote large-scale green and high-value comprehensive utilization.

[0004] The research on the preparation of titanium alloy or nano-titanium dioxide from TBFS mainly has two basic ideas: pyrometallurgy (high temperature carbonization-low temperature chlorination, alkali roasting, metal thermal reduction) and wet method (hydrochloric acid, sulfuric acid). The high temperature carbonization-low temperature chlorination method uses carbon and TBFS as raw materials, and obtains high-purity TiO2 after carbonization at 1580-1700℃, chlorination at 400-600℃, alum removal, distillation, and oxidation. This method is suitable for processing hot TBFS just out of the furnace, and has high requirements for equipment corrosion resistance and difficulty in handling chlorine-containing residues, so it has not yet been industrially applied; the alkali roasting method is to react alkaline substances such as sodium hydroxide with TBFS at 200-700℃, and the product is washed with water, dissolved in acid, hydrolyzed, calcined and other processes to obtain TiO2. This method has large acid and alkali consumption, high sodium salt recovery cost, complicated process flow, and high equipment requirements. It is still in the experimental research and development stage; the metal thermal reduction method uses TBFS as raw material, silicon-iron alloy or silicon-aluminum-iron alloy as reducing agent, and undergoes high temperature melting, recasting and other steps. The method is to prepare titanium-silicon or titanium-iron alloy by a single step. This method has a short process and strong adaptability to raw materials, but it is costly, energy-intensive, and has a small application market. It has not yet been industrialized. The hydrochloric acid method is to mix hydrochloric acid and TBFS at 80-130°C for acid hydrolysis for 4-20 hours, and then filter, distill, hydrolyze at normal pressure, calcine and other processes to obtain TiO2. This method has high requirements for acid concentration (>30%) and equipment corrosion protection, and it is difficult to treat chlorine-containing wastewater. There is no industrial application. The sulfuric acid method is to use sulfuric acid to react with TBFS to obtain titanium oxysulfate (TiOSO4) solution, and then filter, distill, hydrolyze at normal pressure, calcine and other steps to obtain TiO2. The sulfuric acid method for treating TBFS mainly includes liquid phase method and solid phase method. The sulfuric acid-solid phase method is now widely used in the industrial production of titanium dioxide from ilmenite. Therefore, this method for treating TBFS to prepare TiO2 has great application potential.

[0005] Chinese patent document CN117865217A discloses a method for preparing titanium dioxide using titanium-rich material as raw material, comprising: step S1, roasting and leaching titanium-containing blast furnace slag under pressure with nitric acid, and then performing solid-liquid separation to obtain blast furnace slag leachate and titanium-rich material; step S2, fully mixing the titanium-rich material with concentrated sulfuric acid and adding an appropriate amount of water, and then performing heat preservation roasting under low temperature conditions to form a loose and porous solid phase; step S3, adding an appropriate amount of water to the solid phase, heating and stirring to leach, and obtaining a leachate and a leachate through solid-liquid separation; step S4, preparing titanium dioxide through the leachate through processes such as concentration, reduction, hydrolysis, and roasting.

[0006] In the existing sulfuric acid-solid phase method, the titanyl sulfate solution obtained from titanium-containing blast furnace slag is significantly different from the industrial standard, mainly in the following aspects: low titanium concentration, the titanium content in the solution (in terms of TiO2) is usually less than 120g / L; high impurity content, magnesium sulfate (MgSO4) concentration exceeds 20g / L, aluminum sulfate [Al2(SO4)3] concentration also exceeds 20g / L; process limitations, due to the limitations of atmospheric pressure hydrolysis conditions, this low-concentration, high-impurity titanium liquid cannot be directly hydrolyzed, and needs to be purified and concentrated before atmospheric pressure self-generation or external seed hydrolysis operation. These characteristics lead to a series of problems such as long production process, high energy consumption, and low titanium recovery rate. Therefore, this method faces many challenges in industrial applications and is difficult to promote widely. To make it have practical application value, further technical improvements and innovations are needed. Summary of the invention

[0007] In order to solve the deficiencies in the prior art, the object of the present invention is to provide a high-purity titanium dioxide and a preparation method thereof, which can effectively remove impurities in titanium-containing blast furnace slag, improve the product quality of the obtained titanium dioxide, reduce the amount of acid used, and reduce the risk of environmental pollution.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] A high-purity titanium dioxide and a preparation method thereof, comprising the following steps:

[0010] (1) crushing, grinding and sieving titanium-containing blast furnace slag;

[0011] (2) mixing the sieved titanium-containing blast furnace slag with a sulfuric acid solution, adding a modified complexing agent and a surfactant, and heating the mixture to obtain an acid-hydrolyzed slag; adding the acid-hydrolyzed slag into deionized water, stirring and mixing, and filtering to obtain a solution containing impure sulfuric acid titanium oxide;

[0012] (3) adding the impurity sulfate-containing titanyl solution into a reaction kettle, sealing the reaction kettle, cooling the product, filtering to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0013] (4) Mixing hydrothermal metatitanic acid and NaOH solution to form a slurry, adjusting the pH, stirring at room temperature, filtering, washing, and drying the product to obtain desulfurized metatitanic acid; calcining the desulfurized metatitanic acid, and cooling to obtain the high-purity titanium dioxide.

[0014] Preferably, in step (1), the product is sieved through a 200-600 mesh sieve.

[0015] Preferably, in step (2), the concentration of the sulfuric acid solution is 85-98 wt %; the heating reaction conditions are 70-130° C. for 1-6 hours; and the surfactant is one or more of anionic surfactants and nonionic surfactants.

[0016] Preferably, in step (2), the dosage ratio of titanium-containing blast furnace slag and sulfuric acid solution is 1:1.5-2.2; the dosage of modified complexing agent and surfactant is 0.01-0.5wt% and 0.5-2wt% of the titanium-containing blast furnace slag, respectively; and the dosage ratio of acid hydrolysis slag and deionized water is 1:1-2.

[0017] Preferably, in step (3), the sealed reaction conditions are hydrothermal reaction at 110-160° C. and 0.2-1 MPa for 1-12 h.

[0018] Preferably, in step (4), the concentration of NaOH solution is 0.5-5wt%, and the pH is adjusted to 10-14; the stirring conditions at room temperature are stirring at 400-800r / min for 30-120min, the drying conditions are drying at 100-110°C for 1-3h; and the calcination conditions are calcining in a muffle furnace at 500-1000°C for 2-5h.

[0019] Preferably, in step (2), the structural formula of the modified complexing agent is one of Formula I or Formula II:

[0020]

[0021] More preferably, in step (2), the structural formula of the modified complexing agent is as follows:

[0022]

[0023] Preferably, in step (2), the method for preparing the modified complexing agent comprises the following steps:

[0024] Add iminodiacetic acid and potassium carbonate to tetrahydrofuran, slowly add trimesoyl chloride dropwise under ice bath condition, stir to react under ice bath condition, remove the solvent tetrahydrofuran by rotary evaporation, then add ethyl acetate for extraction and separation, rotary evaporation, recrystallize the product in ethyl acetate to obtain the modified complexing agent.

[0025] Preferably, the molar ratio of the iminodiacetic acid, potassium carbonate and trimesoyl chloride is 1:2.5-4:2-3.1.

[0026] Preferably, the trimesoyl chloride is added dropwise over 30 to 90 minutes, and the stirring reaction condition is 0 to 5° C. for 1 to 6 hours.

[0027] Under ice bath conditions (0-5°C), iminodiacetic acid and potassium carbonate are mixed in tetrahydrofuran solvent, and then trimesoyl chloride is slowly added dropwise, and the reaction is continued to be stirred in the ice bath. After the reaction is completed, the tetrahydrofuran solvent is removed by a rotary evaporator, and then the product is extracted and separated with ethyl acetate, and then the ethyl acetate is removed again by a rotary evaporator, and finally recrystallized with ethyl acetate to obtain the final product modified complexing agent.

[0028] The core of this reaction is the acylation reaction between the acyl chloride and the amino group to generate N-substituted amide. Trimesoyl chloride contains three acyl chloride groups, which can react with the secondary amine group in iminodiacetic acid to undergo acylation. The acylation reaction in this step is carried out in a low temperature ice bath environment to slow down the reaction rate, thereby increasing the product yield and reducing the occurrence of side reactions. Slowly adding trimesoyl chloride can ensure that the reaction is more thorough and avoid local excess leading to increased side reactions.

[0029] As an alkaline substance, potassium carbonate not only removes acidic impurities in the raw materials, but also provides the alkaline environment required for the reaction, promoting the reaction. In this process, potassium carbonate neutralizes the by-products produced during the reaction, such as hydrochloric acid, ensuring that the reaction medium remains alkaline.

[0030] In the post-processing stage after the reaction is completed, the tetrahydrofuran solvent is removed by a rotary evaporator (rotary evaporation) to obtain a preliminary product. Subsequently, the reaction mixture is extracted with ethyl acetate to separate non-polar impurities, and the ethyl acetate is removed by rotary evaporation to obtain the refined product required for recrystallization. Finally, the product is further purified by recrystallization in ethyl acetate to ensure that the final modified complexing agent has a high purity.

[0031] The present invention also claims to protect high-purity titanium dioxide prepared by the preparation method.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1) The present invention provides a high-purity titanium dioxide and a preparation method thereof. The high-purity titanium dioxide is obtained by crushing, acidolysis, hydrothermal reaction and roasting with titanium-containing blast furnace slag as raw material, and is suitable for multiple industries such as coatings, plastics, and papermaking. Adding a surfactant during the acidolysis process can effectively prevent the agglomeration and sedimentation of the titanium-containing blast furnace slag, solubilize the insoluble impurities, and improve the reaction efficiency of the slag with sulfuric acid and a modified complexing agent. The method provided by the present invention can effectively remove impurities in the titanium-containing blast furnace slag, improve the product quality of the obtained titanium dioxide, reduce the amount of acid used, and reduce the risk of environmental pollution.

[0034] 2) The present invention provides a modified complexing agent, which contains multiple carboxyl functional groups and can selectively form stable complexes with impurity ions such as alkali metals and alkaline earth metals in blast furnace slag, significantly improving the solubility of impurities in acidic solutions, and helping to efficiently separate impurities from titanium-containing blast furnace slag to obtain purer titanium products. Compared with the traditional strong acid leaching process, the use of modified complexing agents can reduce the amount of acid used, reduce the risk of environmental pollution, and also play an important role in improving product quality and process efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show schematic diagrams of certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 This is a SEM photograph of the high-purity titanium dioxide prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0038] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.

[0039] The titanium-containing blast furnace slag used in the embodiments and comparative examples comes from a domestic factory, and its chemical composition is shown in Table 1:

[0040] Table 1 Main composition of titanium-containing blast furnace slag

[0041]

[0042] A method for preparing high-purity titanium dioxide comprises the following steps:

[0043] (1) adding 10 mmol of iminodiacetic acid and 2.5-4 mmol of potassium carbonate to 50 mL of tetrahydrofuran, slowly adding 2-3.1 mmol of trimesoyl chloride dropwise under ice bath conditions for 30-90 min, stirring and reacting under ice bath conditions of 0-5° C. for 1-6 h, removing the solvent tetrahydrofuran from the product by rotary evaporation, then adding ethyl acetate for extraction and separation, rotary evaporation, and recrystallizing the product in ethyl acetate to obtain the modified complexing agent;

[0044] (2) crushing and grinding the titanium-containing blast furnace slag and passing it through a 200-600 mesh sieve;

[0045] (3) 1 kg of sieved titanium-containing blast furnace slag is mixed with 1.55-2.2 kg of 85-98 wt% sulfuric acid solution, and 0.1-5 g of a modified complexing agent and 5-20 g of a surfactant are added, and the mixture is reacted at 70-130° C. for 1-6 h to obtain an acid-hydrolyzed slag; 1 kg of the acid-hydrolyzed slag is added to 1-2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing miscellaneous sulfuric acid titanium oxide;

[0046] (4) adding the titanium dioxide solution containing impurity sulfate into a reaction kettle, conducting a sealed hydrothermal reaction at 110-160° C. and 0.2-1 MPa for 1-12 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0047] (5) Mixing hydrothermal titanic acid with 0.5-5wt% NaOH solution to form a slurry, adjusting the pH to 10-14, stirring at room temperature at 400-800 r / min for 30-120 min, filtering the product, washing, and drying at 100-110°C for 1-3 h to obtain desulfurized titanic acid; calcining the desulfurized titanic acid at 500-1000°C in a muffle furnace for 2-5 h, and cooling to obtain the high-purity titanium dioxide.

[0048] The present invention will be further described below through specific embodiments.

[0049] Example 1

[0050] A method for preparing high-purity titanium dioxide comprises the following steps:

[0051] (1) adding 10 mmol of iminodiacetic acid and 4 mmol of potassium carbonate to 50 mL of tetrahydrofuran, slowly adding 3.1 mmol of trimesoyl chloride (dissolved in 10 mL of tetrahydrofuran in advance) dropwise under ice bath conditions, the addition is completed over 90 min, stirring in an ice bath for 1 h, the product is rotary evaporated to remove the solvent tetrahydrofuran, then ethyl acetate is added for extraction and separation, rotary evaporated, and the product is recrystallized in ethyl acetate to obtain the modified complexing agent;

[0052] (2) crushing and grinding the titanium-containing blast furnace slag and passing it through a 500-mesh sieve;

[0053] (3) 1 kg of sieved titanium-containing blast furnace slag was mixed with 2.2 kg of 85 wt% sulfuric acid solution, and 5 g of a modified complexing agent and 20 g of a surfactant, sodium hexadecylbenzene sulfonate, were added, and the mixture was reacted at 130° C. for 1 h to obtain an acid-hydrolyzed slag; 1 kg of the acid-hydrolyzed slag was added to 2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0054] (4) adding the impurity sulfate-containing titanyl solution into a reaction kettle, conducting a sealed hydrothermal reaction at 160° C. and 1 MPa for 1 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0055] (5) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature at 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 600°C in a muffle furnace for 4 h, cool and obtain anatase-type high-purity titanium dioxide with a purity of 99.5%.

[0056] The SEM photo of the anatase titanium dioxide prepared in Example 1 is as follows Figure 1 shown.

[0057] Example 2

[0058] A method for preparing high-purity titanium dioxide comprises the following steps:

[0059] (1) adding 10 mmol of iminodiacetic acid and 3 mmol of potassium carbonate to 50 mL of tetrahydrofuran, slowly adding 2.5 mmol of trimesoyl chloride (dissolved in 10 mL of tetrahydrofuran in advance) dropwise under ice bath conditions, the addition is completed over 60 min, stirring and reacting under ice bath conditions for 3 h, removing the solvent tetrahydrofuran from the product by rotary evaporation, then adding ethyl acetate for extraction and separation, rotary evaporation, and recrystallizing the product in ethyl acetate to obtain the modified complexing agent;

[0060] (2) crushing and grinding the titanium-containing blast furnace slag and passing it through a 400-mesh sieve;

[0061] (3) 1 kg of sieved titanium-containing blast furnace slag was mixed with 1.9 kg of 93 wt% sulfuric acid solution, and 2.5 g of a modified complexing agent and 12 g of a surfactant, sodium hexadecylbenzene sulfonate, were added, and the mixture was reacted at 100° C. for 3 h to obtain an acid-hydrolyzed slag; 1 kg of the acid-hydrolyzed slag was added to 1.5 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0062] (4) adding the impurity sulfate-containing titanyl solution into a reaction kettle, conducting a sealed hydrothermal reaction at 130° C. and 0.6 MPa for 6 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0063] (5) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature at 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 600°C in a muffle furnace for 4 h, cool and obtain anatase-type high-purity titanium dioxide with a purity of 99.4%.

[0064] Example 3

[0065] A method for preparing high-purity titanium dioxide comprises the following steps:

[0066] (1) adding 10 mmol of iminodiacetic acid and 2.5 mmol of potassium carbonate to 50 mL of tetrahydrofuran, slowly adding 2.1 mmol of trimesoyl chloride (dissolved in 10 mL of tetrahydrofuran in advance) dropwise under ice bath conditions, the addition is completed over 30 min, stirring in an ice bath for 6 h, the product is rotary evaporated to remove the solvent tetrahydrofuran, then ethyl acetate is added for extraction and separation, rotary evaporated, and the product is recrystallized in ethyl acetate to obtain the modified complexing agent;

[0067] (2) crushing and grinding the titanium-containing blast furnace slag and passing it through a 400-mesh sieve;

[0068] (3) 1 kg of sieved titanium-containing blast furnace slag was mixed with 1.55 kg of 85 wt% sulfuric acid solution, and 1 g of a modified complexing agent and 5 g of a surfactant, sodium hexadecylbenzene sulfonate, were added, and the mixture was reacted at 70° C. for 6 h to obtain an acid-hydrolyzed slag; 1 kg of the acid-hydrolyzed slag was added to 1 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0069] (4) adding the impurity sulfate-containing titanyl solution into a reaction kettle, sealing and hydrothermally reacting the mixture at 110° C. and 0.2 MPa for 12 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0070] (5) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature and 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 500°C in a muffle furnace for 5 h, cool and obtain anatase-type high-purity titanium dioxide with a purity of 99.2%.

[0071] Example 4

[0072] A method for preparing high-purity titanium dioxide comprises the following steps:

[0073] (1) adding 10 mmol of iminodiacetic acid and 3 mmol of potassium carbonate to 50 mL of tetrahydrofuran, slowly adding 2.5 mmol of trimesoyl chloride (dissolved in 10 mL of tetrahydrofuran in advance) dropwise under ice bath conditions, the addition is completed over 60 min, stirring and reacting under ice bath conditions for 3 h, removing the solvent tetrahydrofuran from the product by rotary evaporation, then adding ethyl acetate for extraction and separation, rotary evaporation, and recrystallizing the product in ethyl acetate to obtain the modified complexing agent;

[0074] (2) crushing and grinding the titanium-containing blast furnace slag and passing it through a 400-mesh sieve;

[0075] (3) 1 kg of sieved titanium-containing blast furnace slag was mixed with 1.9 kg of 93 wt% sulfuric acid solution, and 2.5 g of a modified complexing agent and 12 g of a surfactant, sodium hexadecylbenzene sulfonate, were added, and the mixture was reacted at 100° C. for 3 h to obtain an acid-hydrolyzed slag; 1 kg of the acid-hydrolyzed slag was added to 1.5 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0076] (4) adding the impurity sulfate-containing titanyl solution into a reaction kettle, conducting a sealed hydrothermal reaction at 130° C. and 0.6 MPa for 6 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0077] (5) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature at 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 900°C in a muffle furnace for 3 h, cool and obtain rutile high-purity titanium dioxide with a purity of 99.3%.

[0078] Comparative Example 1

[0079] A method for preparing titanium dioxide using titanium-containing blast furnace slag comprises the following steps:

[0080] (1) crushing and grinding titanium-containing blast furnace slag and passing through a 500-mesh sieve;

[0081] (2) 1 kg of sieved titanium-containing blast furnace slag was mixed with 2.2 kg of 85 wt% sulfuric acid solution, and 5 g of complexing agent iminodiacetic acid and 20 g of surfactant sodium hexadecylbenzenesulfonate were added, and the mixture was reacted at 130° C. for 1 h to obtain acid hydrolysis residue; 1 kg of the acid hydrolysis residue was added into 2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0082] (3) adding the titanium dioxide solution containing impurity sulfate into a reaction kettle, conducting a sealed hydrothermal reaction at 160° C. and 1 MPa for 1 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0083] (4) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature and 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 700°C in a muffle furnace for 4 h, cool and obtain anatase titanium dioxide with a purity of 98.1%.

[0084] Comparative Example 2

[0085] A method for preparing titanium dioxide using titanium-containing blast furnace slag comprises the following steps:

[0086] (1) crushing and grinding titanium-containing blast furnace slag and passing through a 500-mesh sieve;

[0087] (2) 1 kg of sieved titanium-containing blast furnace slag was mixed with 2.2 kg of 85 wt% sulfuric acid solution, and 5 g of chelating agent ethylenediaminetetraacetic acid and 20 g of surfactant sodium hexadecylbenzenesulfonate were added, and the mixture was reacted at 130° C. for 1 h to obtain acid hydrolysis slag; 1 kg of the acid hydrolysis slag was added into 2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0088] (3) adding the titanium dioxide solution containing impurity sulfate into a reaction kettle, conducting a sealed hydrothermal reaction at 160° C. and 1 MPa for 1 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0089] (4) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature at 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 700°C in a muffle furnace for 4 h, cool and obtain anatase titanium dioxide with a purity of 98.2%.

[0090] Comparative Example 3

[0091] A method for preparing high-purity titanium dioxide comprises the following steps:

[0092] (1) adding 10 mmol of iminodiacetic acid and 4 mmol of potassium carbonate to 50 mL of tetrahydrofuran, slowly adding 3.1 mmol of trimesoyl chloride (dissolved in 10 mL of tetrahydrofuran in advance) dropwise under ice bath conditions, the addition is completed over 90 min, stirring in an ice bath for 1 h, the product is rotary evaporated to remove the solvent tetrahydrofuran, then ethyl acetate is added for extraction and separation, rotary evaporated, and the product is recrystallized in ethyl acetate to obtain the modified complexing agent;

[0093] (2) crushing and grinding the titanium-containing blast furnace slag and passing it through a 500-mesh sieve;

[0094] (3) 1 kg of sieved titanium-containing blast furnace slag was mixed with 2.2 kg of 85 wt% sulfuric acid solution, and 5 g of a modified complexing agent was added, and the mixture was reacted at 130° C. for 1 h to obtain an acid-hydrolyzed slag; 1 kg of the acid-hydrolyzed slag was added to 2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0095] (4) adding the impurity sulfate-containing titanyl solution into a reaction kettle, conducting a sealed hydrothermal reaction at 160° C. and 1 MPa for 1 h, cooling and filtering the product to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0096] (5) Mix hydrothermal titanic acid with 3 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature at 600 r / min for 90 min, filter, wash and dry the product at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid at 700°C in a muffle furnace for 4 h, cool and obtain anatase-type high-purity titanium dioxide with a purity of 98.9%.

[0097] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing high-purity titanium dioxide, characterized in that: The steps include: (1) crushing, grinding and sieving titanium-containing blast furnace slag; (2) mixing the sieved titanium-containing blast furnace slag with a sulfuric acid solution, adding a modified complexing agent and a surfactant, and heating the mixture to obtain an acid-hydrolyzed slag; adding the acid-hydrolyzed slag into deionized water, stirring and mixing, and filtering to obtain a solution containing impure sulfuric acid titanium oxide; (3) adding the impurity sulfate-containing titanyl solution into a reaction kettle, sealing the reaction kettle, cooling the product, filtering to obtain a filter cake, washing and drying the filter cake to obtain hydrothermal metatitanic acid; (4) mixing hydrothermal metatitanic acid and NaOH solution to form a slurry, adjusting the pH, stirring at room temperature, filtering, washing, and drying the product to obtain desulfurized metatitanic acid; The desulfurized metatitanic acid is calcined and cooled to obtain the high-purity titanium dioxide.

2. The preparation method according to claim 1, characterized in that: In step (1), the product is sieved through a 200-600 mesh sieve.

3. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the sulfuric acid solution is 85-98 wt %; the heating reaction conditions are 70-130° C. for 1-6 hours; and the surfactant is one or more of anionic surfactants and nonionic surfactants.

4. The preparation method according to claim 1, characterized in that: In step (2), the dosage ratio of titanium-containing blast furnace slag and sulfuric acid solution is 1:1.5-2.2; the dosage of modified complexing agent and surfactant is 0.01-0.5wt% and 0.5-2wt% of the titanium-containing blast furnace slag respectively; the dosage ratio of acid hydrolysis slag and deionized water is 1:1-2.

5. The preparation method according to claim 1, characterized in that: In step (3), the sealed reaction conditions are hydrothermal reaction at 110-160° C. and 0.2-1 MPa for 1-12 hours.

6. The preparation method according to claim 1, characterized in that: In step (4), the concentration of NaOH solution is 0.5-5wt%, and the pH is adjusted to 10-14; the stirring condition at room temperature is stirring at 400-800r / min for 30-120min, the drying condition is drying at 100-110°C for 1-3h; and the calcination condition is calcining in a muffle furnace at 500-1000°C for 2-5h.

7. The preparation method according to claim 1, characterized in that: In step (2), the preparation method of the modified complexing agent comprises the following steps: Add iminodiacetic acid and potassium carbonate to tetrahydrofuran, slowly add trimesoyl chloride dropwise under ice bath condition, stir to react under ice bath condition, remove the solvent tetrahydrofuran by rotary evaporation, then add ethyl acetate for extraction and separation, rotary evaporation, recrystallize the product in ethyl acetate to obtain the modified complexing agent.

8. The preparation method according to claim 7, characterized in that: The molar ratio of the iminodiacetic acid, potassium carbonate and trimesoyl chloride is 1:2.5-4:2-3.

1.

9. The preparation method according to claim 7, characterized in that: The trimesoyl chloride is added dropwise over 30 to 90 minutes, and the reaction is stirred at 0 to 5°C for 1 to 6 hours.

10. High-purity titanium dioxide prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing high-purity titanium pigment by using high-purity water

    CN101973580A

  • Method for preparing high-purity titanium dioxide from titanium-containing blast furnace slag

    CN112047377A