Method for deeply removing impurities from waste SCR (Selective Catalytic Reduction) catalyst
Through mechanochemical synergistic strengthening technology, deep removal of As elements and efficient recovery of V/W in waste SCR catalysts, the problem of removing impurity elements is solved, and new materials are provided for the preparation of new SCR catalysts, simplifying the process flow and reducing energy This has achieved efficient utilization of resources and environmental protection.
Patent Information
- Application Number
- CN202411105415.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has the problem of efficient removal of impurity elements in the resource utilization of waste SCR catalysts, which leads to the inability to recycle the carrier titanium dioxide, and the recycling process is complex, energy consumption is high, and there is environmental risk.
Using mechanochemical synergistic strengthening methods, the toxic component As in the catalyst is deeply removed through ash cleaning and pretreatment and mechanochemical strengthening of alkali liquid, the toxic component As in the catalyst is achieved, and the efficient leaching of the valuable element V/W is achieved, and high-quality titanium dioxide is obtained. body.
The deep removal of poisoned components As in waste SCR catalysts and efficient recycling of valuable metal elements V/W are achieved, and new materials are provided for the preparation of new SCR catalysts, which simplifies the process flow, reduces energy consumption and avoids The generation of secondary solid waste and waste liquid has enhanced the value of resource utilization.
Smart Images

Figure CN118929747A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic chemical technology, and relates to the technical fields of physical pretreatment of hazardous solid waste, efficient leaching of valuable metal elements, preparation of Ti / W / V high-value products, and more specifically to a method for deep removal of impurities from waste SCR catalysts. Background Art
[0002] Coal-fired power generation is the main force of China's electricity production. In order to achieve emission reduction and control of combustion pollutants, most coal-fired power plants use selective catalytic reduction (SCR) to control nitrogen oxides (NOX) in the flue gas during the coal combustion process.
[0003] The commercial SCR denitrification catalyst widely used at present mainly uses anatase TiO2 as a carrier, V2O5 as an active component, and WO3 as an active additive. The denitrification activity of the catalyst gradually decreases with the increase of operating time. The reasons for the decrease in catalyst activity are divided into physical deactivation and chemical deactivation. Physical deactivation mainly includes structural collapse, ash accumulation blockage, sintering deactivation, etc. Chemical deactivation mainly includes active component loss, chemical substance blockage, chemical substance poisoning, etc. Generally, SCR catalysts need to be replaced after 3 to 5 years of continuous operation. The composition of waste SCR denitrification catalysts is complex. During the flue gas denitrification process, toxic components such as As will be loaded in the catalyst. From a resource perspective, waste SCR catalysts contain a certain amount of valuable metal elements such as Ti, W, and V. The comprehensive disposal and utilization of them will produce dual benefits of environmental protection and economic benefits. Combined with the current status of comprehensive disposal of waste SCR catalysts, the direct recovery process has the problems of resource waste and environmental risks. The separation recovery process has the advantages of high resource utilization, but it has the disadvantages of complex disposal process routes and high process material consumption and energy consumption. Therefore, the development of green and efficient recycling technology for waste SCR denitrification catalysts is of great significance for their resource utilization and harmless disposal.
[0004] In the process of resource utilization of waste SCR catalysts, the efficient removal of impurity elements and the recovery of the physical structure properties of the powder are the core key points that people pay attention to. At present, the high-temperature and high-alkali reaction system is mainly used for the efficient removal of impurity elements to achieve efficient removal of impurity elements. CN 116219157A discloses a method for recovering vanadium, tungsten and titanium from waste SCR catalysts by low-temperature sodium calcination. The calcination temperature in the method is 500℃~600℃, and the calcination time is 0.8~1.2h. The calcined material is obtained, and after wet leaching, a leaching liquid containing vanadium and tungsten is obtained. CN 113198457A discloses a medium-low temperature denitration catalyst prepared from waste SCR catalysts and a preparation method. The waste SCR catalysts are dedusted and cleaned, and the crushed waste SCR catalysts are mixed with a molding aid to prepare a honeycomb carrier. CN 110923459A discloses a method for recovering titanium tungsten powder from waste SCR catalyst, wherein the waste SCR catalyst is ground and then sieved to obtain waste catalyst powder with a particle size of less than 5 μm; then oxalic acid acid leaching, hydrofluoric acid acid leaching and sulfuric acid solution acid leaching are respectively added in three steps, wherein arsenic oxide and silicon dioxide are removed, and finally a titanium sulfate solution is obtained by filtration, a surfactant is added thereto, and after precipitation with ammonia water, impurities are removed together with the filter residue to remove Fe, K and Na, and high-temperature calcination is performed and the titanium tungsten powder is obtained by grinding. CN 112718778A discloses a method for deep arsenic removal in an acidic system of waste SCR catalyst, wherein a cleaning solution containing an acidic substance and an auxiliary agent is used to achieve the simultaneous removal of toxic components such as arsenic, potassium, sodium and iron, and the removal rate can reach more than 95%, and the content of the above toxic components in the product is all less than 200ppm. CN110385044A discloses a method for removing arsenic and silicon from waste SCR catalysts. Arsenic and silicon in waste SCR catalysts can be effectively removed by adding additives to alkaline solution. The removal rate of arsenic reaches more than 95%, and the removal rate of silicon can reach more than 50%. CN 111468102A discloses a method for recycling waste SCR denitration catalysts. Acidic cleaning liquid is used to clean and filter the waste SCR denitration catalysts, and an acid hydrolysis reaction is carried out in a sulfuric acid system. After solid-liquid separation, a filter cake is obtained, and then titanium tungsten powder is obtained by drying and calcining. The ideas and methods proposed by the above research units have obtained titanium dioxide carriers and V / W series products with good physical and chemical performance. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for deep removal of impurities from waste SCR catalysts. The present invention utilizes the means of mechanochemical synergistic strengthening to solve the problem that the carrier titanium dioxide cannot be recycled due to contamination by the impurity As, and provides new materials for the preparation of new SCR catalysts; at the same time, the valuable elements V / W in the waste SCR catalysts are efficiently leached, thereby improving the economic utilization value of the waste SCR catalysts.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for deep removal of impurities from a waste SCR catalyst, the method comprising the following steps:
[0008] (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst;
[0009] (2) mixing the alkali solution and the cleaned waste catalyst obtained in step (1) and sequentially subjecting the mixed alkali solution to mechanochemical enhanced leaching and solid-liquid separation to obtain leaching residue and leaching solution;
[0010] (3) The leached residue obtained in step (2) is sequentially washed, solid-liquid separated and dried to obtain titanium dioxide.
[0011] The present invention uses waste SCR catalyst as raw material, pre-treats the waste SCR catalyst through ash cleaning, physically removes a large amount of fly ash that blocks the pores, and then uses the means of mechanical and chemical synergistic strengthening to deeply remove the poisonous component As element inside the waste SCR catalyst, and efficiently leaches the valuable element V / W. After the purification treatment, the main mineral phase composition of the carrier is anatase titanium dioxide, which solves the problem that the carrier titanium dioxide cannot be recycled due to contamination by impurity As, and provides new materials for the preparation of new SCR catalysts; at the same time, the valuable element V / W in the waste SCR catalyst is efficiently leached, thereby improving the economic utilization value of the waste SCR catalyst.
[0012] As a preferred technical solution of the present invention, the cleaning pretreatment in step (1) includes: dry physical cleaning and / or wet cleaning.
[0013] Preferably, the dry physical cleaning comprises: using compressed air for purging.
[0014] Preferably, the pressure of the purging treatment is 0.6-0.8 MPa, for example, 0.6 MPa, 0.64 MPa, 0.68 MPa, 0.72 MPa, 0.76 MPa or 0.8 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0015] Preferably, the wet cleaning comprises: immersing the waste SCR catalyst in a solution and performing ultrasonic cleaning.
[0016] The present invention separates sticky fly ash from waste SCR catalyst by ash cleaning pretreatment, and obtains a mineral phase composition with extremely low fly ash content, wherein the main component of the mineral phase composition is an anatase titanium dioxide carrier.
[0017] As a preferred technical solution of the present invention, the alkali solution in step (2) includes sodium hydroxide and / or potassium hydroxide.
[0018] Preferably, the concentration of the alkali solution in step (2) is 3 to 20 wt%, for example, 3 wt%, 5 wt%, 8 wt%, 11 wt%, 14 wt%, 17 wt% or 20 wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the liquid-to-solid ratio of the alkali solution and the cleaned waste catalyst is 2 to 5 mL:1 g, for example, it can be 2 mL:1 g, 2.5 mL:1 g, 3 mL:1 g, 3.5 mL:1 g, 4 mL:1 g, 4.5 mL:1 g or 5 mL:1 g, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] As a preferred technical solution of the present invention, the temperature of the mechanochemical enhanced leaching in step (2) is 20 to 90°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] Preferably, the time for the mechanochemical enhanced leaching in step (2) is 0.5 to 2 h, for example, 0.5 h, 0.8 h, 1.1 h, 1.4 h, 1.7 h or 2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] Preferably, the mechanochemical enhanced leaching in step (2) is accompanied by mechanical grinding.
[0023] The mechanochemical enhanced leaching of the present invention is specifically as follows: mechanical grinding is performed while leaching with alkali solution, and the formation of by-products such as sodium titanate is avoided by limiting the alkali solution concentration, alkali solution dosage and leaching temperature during the leaching process, thereby achieving efficient leaching of poisonous components (As) and valuable elements (V / W) in the powder; if the alkali solution concentration is too high, the by-product sodium titanate will be generated, affecting the quality and yield of titanium dioxide; if the leaching temperature is too high, the by-product sodium titanate will be generated, and at the same time, the high temperature will increase the dissolution rate of titanium dioxide and reduce the powder yield; if the leaching temperature is too low, the impurity removal effect will be poor, and the impurity As element is difficult to be deeply removed.
[0024] As a preferred technical solution of the present invention, the equipment used for the mechanochemical enhanced leaching in step (2) includes any one of a ball mill, a rod mill or a sand mill, preferably a ball mill.
[0025] Preferably, the leaching solution in step (2) is a mixed solution rich in V and W.
[0026] The present invention can process the leaching solution by means of segmented evaporation and crystallization according to the different physical properties of V and W to obtain sodium vanadate and sodium tungstate.
[0027] As a preferred technical solution of the present invention, the temperature of the washing water used in step (3) is 60-95°C, for example, it can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the liquid-to-solid ratio of washing water to leached residue in the washing in step (3) is 2 to 5 mL:1 g, for example, 2 mL:1 g, 2.5 mL:1 g, 3 mL:1 g, 3.5 mL:1 g, 4 mL:1 g, 4.5 mL:1 g or 5 mL:1 g, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the washing in step (3) comprises countercurrent washing.
[0030] Preferably, the countercurrent washing is performed 3 to 5 times, for example, 3 times, 4 times or 5 times.
[0031] As a preferred technical solution of the present invention, the washing liquid obtained in step (3) is reused in the dust cleaning pretreatment in step (1).
[0032] In the present invention, the temperature of the washing water used for washing is 60-95°C. If the temperature is too high, the energy consumption of the washing process will increase. At the same time, part of the high-temperature washing water will react with the residual alkali attached to the powder to generate sodium titanate by-product, affecting the quality and yield of the powder product. If the temperature is too low, the washing effect will be poor, and some physically attached impurity elements will be difficult to remove.
[0033] As a preferred technical solution of the present invention, the drying temperature in step (3) is 80-110°C, for example, it can be 80°C, 85°C, 90°C, 95°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] Preferably, the drying time in step (3) is 12 to 24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] As a preferred technical solution of the present invention, the waste SCR catalyst includes a titanium dioxide carrier and V2O5 and WO3 loaded on the titanium dioxide carrier.
[0036] As a preferred technical solution of the present invention, the method for deep removal of impurities from waste SCR catalyst provided by the present invention comprises the following steps:
[0037] (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst;
[0038] (2) mixing an alkali solution having a concentration of 3 to 20 wt% and the clean spent catalyst obtained in step (1) at a liquid-to-solid ratio of 2 to 5 mL: 1 g, and then performing mechanochemical enhanced leaching at 20 to 90° C. for 0.5 to 2 h, and performing solid-liquid separation to obtain leached residue and a mixed solution rich in V and W;
[0039] (3) washing the leached residue obtained in step (2) with washing water at 60-95° C., and drying at 80-110° C. for 12-24 hours after solid-liquid separation to obtain titanium dioxide;
[0040] Among them, the liquid-to-solid ratio of washing water to leaching residue is 2-5mL:1g.
[0041] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] (1) The present invention achieves deep removal of poisonous component As in the waste SCR catalyst and efficient recovery of valuable metal elements such as V / W by mechanically active synergistically enhancing leaching of waste SCR catalyst and alkali solution, and obtains titanium dioxide powder that can be used to prepare new SCR catalyst, thereby alleviating the shortage of high-quality titanium resources;
[0044] (2) The method provided by the present invention uses waste SCR catalyst as raw material and uses mechanical and chemical synergistic enhanced decontamination to efficiently separate impurities, valuable elements and carriers. The process is simple and the operation is flexible, achieving the common development of economic and environmental benefits.
[0045] (3) Compared with the traditional impurity removal and extraction process, the method provided by the present invention consumes less energy and material, and does not generate secondary solid waste and waste liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a flow chart of the method for deep removal of impurities from waste SCR catalysts provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0048] Example 1
[0049] This embodiment provides a method for deep removal of impurities from waste SCR catalysts, such as Figure 1 As shown, the method comprises the following steps:
[0050] (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst;
[0051] (2) in a ball mill, mixing sodium hydroxide having a concentration of 5 wt% and the clean spent catalyst obtained in step (1) at a liquid-solid ratio of 3 mL:1 g, and then performing mechanochemical enhanced leaching at 90° C. for 1 h, solid-liquid separation, and obtaining leached residue and a mixed solution rich in V and W;
[0052] (3) washing the leached residue obtained in step (2) with washing water at 60° C., and drying at 100° C. for 18 h after solid-liquid separation to obtain titanium dioxide;
[0053] Among them, the liquid-to-solid ratio of washing water to leaching residue is 3mL:1g.
[0054] Example 2
[0055] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst, the method comprising the following steps:
[0056] (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst;
[0057] (2) in a ball mill, mixing sodium hydroxide having a concentration of 8 wt % and the clean spent catalyst obtained in step (1) at a liquid-solid ratio of 5 mL:1 g, and then performing mechanochemical enhanced leaching at 80° C. for 2 h, solid-liquid separation, and obtaining leached residue and a mixed solution rich in V and W;
[0058] (3) washing the leached residue obtained in step (2) with washing water at 65° C., and drying at 80° C. for 24 h after solid-liquid separation to obtain titanium dioxide;
[0059] Among them, the liquid-to-solid ratio of washing water to leaching residue is 5mL:1g.
[0060] Example 3
[0061] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst, the method comprising the following steps:
[0062] (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst;
[0063] (2) in a ball mill, mixing sodium hydroxide having a concentration of 6 wt% and the clean spent catalyst obtained in step (1) at a liquid-solid ratio of 4 mL:1 g, and then performing mechanochemical enhanced leaching at 60° C. for 1.5 h, solid-liquid separation, and obtaining leached residue and a mixed solution rich in V and W;
[0064] (3) washing the leached residue obtained in step (2) with washing water at 65° C., and drying at 110° C. for 12 h after solid-liquid separation to obtain titanium dioxide;
[0065] Among them, the liquid-to-solid ratio of washing water to leaching residue is 4mL:1g.
[0066] Example 4
[0067] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst, the method comprising the following steps:
[0068] (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst;
[0069] (2) In a ball mill, potassium hydroxide having a concentration of 20 wt% and the clean spent catalyst obtained in step (1) are mixed at a liquid-solid ratio of 2 mL:1 g, and then mechanochemical enhanced leaching is performed at 20° C. for 2 h, followed by solid-liquid separation to obtain leached residue and a mixed solution rich in V and W;
[0070] (3) washing the leached residue obtained in step (2) with washing water at 95° C., and drying at 90° C. for 18 h after solid-liquid separation to obtain titanium dioxide;
[0071] Among them, the liquid-to-solid ratio of washing water to leaching residue is 2mL:1g.
[0072] Example 5
[0073] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0074] In this embodiment, the concentration of sodium hydroxide in step (2) is adjusted to 25 wt %.
[0075] Example 6
[0076] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0077] In this embodiment, the concentration of sodium hydroxide in step (2) is adjusted to 35 wt %.
[0078] Example 7
[0079] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0080] In this embodiment, the temperature of the mechanochemical enhanced leaching in step (2) is adjusted to 15°C.
[0081] Example 8
[0082] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0083] In this embodiment, the temperature of the mechanochemical enhanced leaching in step (2) is adjusted to 100°C.
[0084] Example 9
[0085] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0086] In this example, the liquid-to-solid ratio in step (2) was adjusted to 8 mL:1 g.
[0087] Example 10
[0088] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0089] In this embodiment, the temperature of the washing water in step (3) is adjusted to 50°C.
[0090] Embodiment 11
[0091] This embodiment provides a method for deep removal of impurities from a waste SCR catalyst. The method is different from that in Embodiment 1 only in that:
[0092] In this embodiment, the temperature of the washing water in step (3) is adjusted to 100°C.
[0093] Comparative Example 1
[0094] This comparative example provides a method for deep removal of impurities from a waste SCR catalyst, the method differing from Example 1 only in that:
[0095] In this comparative example, the mechanochemical enhanced leaching described in step (2) is adjusted as follows: the clean waste catalyst is first crushed using a planetary ball mill, and then sodium hydroxide with a concentration of 5 wt% and the crushed clean waste catalyst are mixed at a liquid-solid ratio of 3 mL:1 g, and then leaching is performed at 90°C for 1 hour.
[0096] Comparative Example 2
[0097] This comparative example provides a method for deep removal of impurities from a waste SCR catalyst, the method differing from Example 1 only in that:
[0098] In this comparative example, the mechanical grinding process in the mechanochemical strengthening described in step (2) was omitted.
[0099] The content of impurity As in the clean waste catalyst and titanium dioxide powder obtained by the methods provided in the above embodiments and comparative examples was analyzed by X-ray fluorescence spectroscopy. The results are shown in Table 1.
[0100] Table 1
[0101]
[0102] According to Table 1, we can know the following points:
[0103] (1) Comprehensive analysis of Examples 1-4 shows that the method provided by the present invention can effectively achieve deep removal of poisoning component As in waste SCR catalyst, efficiently recover valuable metal elements such as V / W, and obtain titanium dioxide powder that can be used to prepare new SCR catalyst;
[0104] (2) Comprehensive analysis of Example 1 and Examples 5-6 shows that the higher the concentration of the alkali solution during the leaching process, the higher the impurity removal efficiency will be, but the powder yield will decrease as the by-product sodium titanate is generated;
[0105] (3) Comprehensive analysis of Example 1 and Examples 7-8 shows that the temperature limit during the leaching process will affect the impurity removal effect and the powder yield; if the temperature is too high, it will lead to the formation of by-product sodium titanate and reduce the powder yield. If the temperature is too low, the impurity removal effect will be reduced and the residual arsenic content of the powder will increase.
[0106] (4) Comprehensive analysis of Example 1 and Examples 10-11 shows that the temperature of the washing water during the washing process of the leached residue will affect the residual impurity content of the powder and the powder yield; if the temperature is too high, the powder yield will be reduced, and if the temperature is too low, the residual impurity content of the powder will increase;
[0107] (5) Comprehensive analysis of Example 1 and Comparative Examples 1-2 shows that the grinding process during the leaching process has a significant impact on the leaching effect;
[0108] Among them, in comparative example 1, the mechanical and chemical synergistic enhanced leaching was separated, and the physical crushing of the clean waste catalyst and the wet leaching of impurities were processed in steps. Since the simple physical and mechanical crushing can only reduce the particle size of the carrier, the leaching process cannot effectively remove the As embedded in the titanium dioxide lattice, resulting in a high residual As content in the purified slag, and the efficient removal of impurity elements cannot be achieved;
[0109] In Comparative Example 2, the grinding process in the leaching process was omitted, resulting in that the impurity elements could not fully contact with the reaction medium, and the mass transfer process limited the effect of the final impurity removal;
[0110] In summary, the method provided by the present invention overcomes the key technical bottleneck of difficult impurity removal, points out that the key to achieving deep impurity removal is that the As element of the waste SCR catalyst is fully contacted with the leaching medium and the resistance of the mass transfer process is reduced. Compared with the traditional process, the energy consumption and material consumption are low, the process is simple, the reaction conditions are mild, the operation flexibility is large, and no secondary solid waste and waste liquid are generated; in addition, the present invention provides a titanium dioxide raw material for the preparation of SCR catalysts, and provides raw materials for the preparation of V / W series products, which alleviates the problem of my country's high dependence on titanium, tungsten and vanadium, and realizes the common development of economic and environmental benefits.
[0111] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for deep removal of impurities from waste SCR catalysts, characterized in that: The method comprises the following steps: (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst; (2) mixing the alkali solution and the cleaned waste catalyst obtained in step (1) and sequentially subjecting the mixed alkali solution to mechanochemical enhanced leaching and solid-liquid separation to obtain leaching residue and leaching solution; (3) The leached residue obtained in step (2) is washed, solid-liquid separated and dried in sequence to obtain titanium dioxide.
2. The method for deep removal of impurities from waste SCR catalyst according to claim 1, characterized in that: The cleaning pretreatment in step (1) includes: dry physical cleaning and / or wet cleaning; Preferably, the dry physical cleaning comprises: using compressed air for purging; Preferably, the wet cleaning comprises: immersing the waste SCR catalyst in a solution and performing ultrasonic cleaning.
3. The method for deep removal of impurities from waste SCR catalyst according to claim 1 or 2, characterized in that: The alkali solution in step (2) includes sodium hydroxide and / or potassium hydroxide; Preferably, the concentration of the alkali solution in step (2) is 3 to 20 wt %; Preferably, the liquid-to-solid ratio of the alkali solution and the cleaned spent catalyst is 2-5 mL:1 g.
4. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 3, characterized in that: The temperature of the mechanochemical enhanced leaching in step (2) is 20 to 90° C. Preferably, the time of the mechanochemical enhanced leaching in step (2) is 0.5 to 2 hours; Preferably, the mechanochemical enhanced leaching in step (2) is accompanied by mechanical grinding.
5. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 4, characterized in that: The equipment used for the mechanochemical enhanced leaching in step (2) includes any one of a ball mill, a rod mill or a sand mill, preferably a ball mill; Preferably, the leaching solution in step (2) is a mixed solution rich in V and W.
6. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 5, characterized in that: The temperature of the washing water used in step (3) is 60-95°C; Preferably, the liquid-to-solid ratio of washing water to leached residue in the washing in step (3) is 2-5 mL:1 g; Preferably, the washing in step (3) comprises countercurrent washing; Preferably, the countercurrent washing is performed 3 to 5 times.
7. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 6, characterized in that: The washing liquid obtained in step (3) is reused in the dust cleaning pretreatment in step (1).
8. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 7, characterized in that: The drying temperature in step (3) is 80-110° C. Preferably, the drying time in step (3) is 12 to 24 hours.
9. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 8, characterized in that: The waste SCR catalyst comprises a titanium dioxide carrier and V2O5 and WO3 loaded on the titanium dioxide carrier.
10. The method for deep removal of impurities from waste SCR catalyst according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) performing dust removal pretreatment on the waste SCR catalyst to obtain a clean waste catalyst; (2) mixing an alkali solution having a concentration of 3 to 20 wt% and the clean spent catalyst obtained in step (1) at a liquid-to-solid ratio of 2 to 5 mL: 1 g, and then performing mechanochemical enhanced leaching at 20 to 90° C. for 0.5 to 2 h, and performing solid-liquid separation to obtain leached residue and a mixed solution rich in V and W; (3) washing the leached residue obtained in step (2) with washing water at 60-95° C., and drying at 80-110° C. for 12-24 hours after solid-liquid separation to obtain titanium dioxide; Among them, the liquid-to-solid ratio of washing water to leaching residue is 2-5mL:1g.