Method for synthesizing ferric oxide mesocrystals by mineralizing ferrihydrite at low temperature

Through the method of mineralizing iron ore to synthesize mesoscopic crystals of iron oxide at near room temperature, the problem of high temperature and high energy consumption of traditional iron oxide preparation is solved, low energy consumption and green iron oxide preparation is realized, and its lithium Good performance in battery negative electrode material.

CN118929771AActive Publication Date: 2024-11-12WUHAN UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411171508.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The preparation of traditional iron oxide requires high temperature conditions, which leads to high preparation costs, high energy consumption and unenvironmental environmentally friendly. The synthesis method of mesoscopic crystals is complicated, making it difficult to achieve green low temperature synthesis.

Method used

The method of synthesis of iron oxide mesogenic crystals by mineralizing iron ore at near room temperature is adopted. By adding iron nitrate nitrate nitrate, ferric chloride and urea to deionized water, and after stirring, cooling, centrifugation and freeze-drying, the Mesooscopic crystals of iron oxide.

Benefits of technology

The low-energy consumption and green preparation of iron oxide are achieved, and the product has a typical mesoscopic crystal structure and good lithium battery performance, simplifying the room temperature preparation technology of biological imitation processes of inorganic materials, and providing new preparation ideas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929771A_ABST
    Figure CN118929771A_ABST
Patent Text Reader

Abstract

The invention relates to a method for synthesizing iron oxide mesocrystals by low-temperature mineralization of ferrihydrite, which comprises the following steps: S1, adding iron nitrate nonahydrate into deionized water, reacting for a period of time under constant-temperature water bath stirring, and cooling to room temperature; centrifugally collecting precipitate, repeatedly washing with deionized water, and finally freeze-drying to obtain ferrihydrite powder; dispersing the ferrihydrite powder into an aqueous solution to obtain a ferrihydrite solution; s2, adding ferric trichloride and urea into deionized water, and continuously stirring to obtain a mineralized solution; dropwise adding a ferrihydrite solution in a continuous stirring state, and continuously stirring to obtain a mixed mineralized solution containing ferrihydrite; putting the reaction kettle filled with the mixed mineralizing solution into a constant-temperature drying oven for full reaction, and then naturally cooling to room temperature; and centrifugally collecting the precipitate, repeatedly washing with deionized water, and finally freeze-drying to obtain the ferric oxide mesocrystal product. The iron oxide mesoscopic crystal material is expected to be applied to the field of energy materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to new materials and application fields thereof, and more specifically to a method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite. Background Art

[0002] Natural materials can complete the structure formation process at room temperature and grow exquisite microstructures, thus having unique functions. This is the result of billions of years of evolution. In modern industry, the preparation methods of materials with similar properties often require high temperatures and other conditions. In recent years, by studying the natural manufacturing process and the relationship between the natural manufacturing process and biological structures, a process bionic preparation technology for materials has been developed, realizing the controllable preparation of inorganic materials at room temperature.

[0003] Jingjing Xie et al. used living clams as a natural biosynthesis platform to synthesize nitrogen-doped anatase TiO2 with a hierarchical pore structure at room temperature, and the powder had excellent photodegradation and photohydrogen production performance. (Jingjing Xie, et al. Mussel-Directed Synthesis of Nitrogen-Doped Anatase TiO2[J]. Angewandte Chemie International Edition, 2016, 55(9): 3031-3035). Wenhao Chi et al. used living clams to synthesize a two-phase uniformly distributed nano SnO2 / graphene oxide composite material at room temperature, which has a high load and good uniformity. In addition, the obtained SnO2 / graphene oxide composite material, as a negative electrode material for lithium-ion batteries, exhibits excellent lithium storage performance. (W Chi, et al. Mussel directed synthesis of SnO2 / graphene oxide composite for energy storage[J]. Materials Chemistry Frontiers, 2021, 5(23): 8238-8247.). Previous studies have shown the feasibility of guiding the room temperature synthesis of inorganic materials based on natural biological platforms. However, the research findings on the room temperature synthesis of inorganic materials in vivo cannot further guide the synthesis of inorganic materials under environmentally friendly conditions in vitro. Therefore, it is necessary to conduct in-depth research on the mechanism of organisms guiding the room temperature synthesis of inorganic materials and the biological functional elements that play a key role in the formation of inorganic materials, and to develop room temperature preparation technology for inorganic materials in the laboratory using biomimetic processes, so as to provide new ideas and approaches for the room temperature synthesis of inorganic functional materials.

[0004] As one of the common functional metal oxides, nano iron oxide shows outstanding performance in light, electricity, magnetism and other aspects, and is widely used in energy, environment and biomedicine. Hematite (α-Fe2O3) is an important member of the iron oxide family, and the preparation of traditional iron oxide often requires higher temperatures. For example, traditional heat treatment to prepare iron oxide often requires more than 250°C, and hydrothermal synthesis of iron oxide requires more than 160°C. In addition, as a functional inorganic oxide material, the structure of its mesoscopic crystals is conducive to improving its application performance. However, the synthesis of iron oxide mesoscopic crystals often requires template etching and high-temperature treatment methods. Therefore, the green preparation of iron oxide mesoscopic crystals is still a major challenge. Organisms can mineralize and synthesize inorganic materials at room temperature and pressure. By learning this biological process, it is expected to innovate the green synthesis method of iron oxide mesoscopic crystals. At the same time, it is of great significance to develop room temperature preparation technology of biomimetic processes that use key biological functional elements in organisms to guide inorganic materials. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite, which utilizes ferrihydrite to mineralize at near room temperature to synthesize iron oxide inorganic materials, has low preparation cost, simple operation, energy saving and environmental protection.

[0006] The technical solution adopted by the present invention to solve the technical problem is: constructing a method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite, comprising the following steps:

[0007] S1. Adding ferric nitrate nonahydrate to deionized water, and then reacting for a period of time in a constant temperature water bath with stirring, and then cooling to room temperature; collecting the precipitate by centrifugation, and repeatedly washing it with deionized water, and finally freeze-drying it to obtain ferrihydrite powder; dispersing the ferrihydrite powder into an aqueous solution to obtain a ferrihydrite solution;

[0008] S2. Add ferric chloride and urea to deionized water, and continue stirring to obtain a mineralized solution; add ferrihydrite solution dropwise under continuous stirring, and continue stirring to obtain a mixed mineralized solution containing ferrihydrite; place the reactor containing the mixed mineralized solution in a constant temperature oven for sufficient reaction and then naturally cool to room temperature; collect the precipitate by centrifugation, wash it repeatedly with deionized water, and finally freeze-dry it to obtain an iron oxide mesoscopic crystal product.

[0009] According to the above scheme, in step S1, the concentration of ferric nitrate nonahydrate in the deionized solution is 8-10 g / L. The concentration of ferrihydrite in the ferrihydrite solution is 5-10 mg / mL;

[0010] According to the above scheme, in step S1, the temperature of the constant temperature water bath is 65-75° C., and the stirring time is 10-12 min.

[0011] According to the above scheme, in step S1, the centrifugal speed is 15000-17000 rpm, the centrifugal time is 10-20 min, the number of deionized water washings is three times, and the freeze-drying time is 24 h.

[0012] According to the above scheme, the concentration of ferric chloride in the mineralization solution is 0.8-1.2 M / L, the concentration of urea is 0.8-1.2 M / L, and the concentration of ferrihydrite in the mixed mineralization solution is 200-600 μg / mL.

[0013] According to the above scheme, in step S2, the stirring time is 10 to 12 minutes.

[0014] According to the above scheme, in step S2, the oven temperature is 60-100° C., and the reaction time is 24-96 hours.

[0015] According to the above scheme, in step S2, the centrifugal speed is 8000-9000 rpm, the centrifugal time is 10-20 min, the number of deionized water washings is three times, and the freeze-drying time is 24 h.

[0016] The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite of the present invention has the following beneficial effects:

[0017] 1. The present invention synthesizes inorganic iron oxide material for the first time at near room temperature using biological functional element ferrihydrite, providing a new preparation method for low energy consumption and green preparation of iron oxide;

[0018] 2. The iron oxide synthesized by the present invention has typical mesoscopic crystal structure characteristics and uniform microscopic morphology, and is expected to be applied in the field of energy materials. The iron oxide mesoscopic crystals obtained under low-temperature mineralization have good lithium battery performance as negative electrode materials for lithium batteries, indicating that the iron oxide has potential application value in energy materials;

[0019] 3. The preparation method of the present invention is simple and easy to operate, and provides an innovative method for the bionic room temperature preparation technology of inorganic materials. The conditions required for preparation are simple, and the particle size of the mineralized product is uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:

[0021] Figure 1 is a transmission electron image of ferrihydrite in Example 1 of the present invention;

[0022] Figure 2 is a scanning electron image of the iron oxide prepared in Example 1 of the present invention;

[0023] Figure 3Transmission electron image, HAADF-STEM image and electron diffraction image of the iron oxide prepared in Example 1 of the present invention;

[0024] Figure 4 The lithium battery cycle performance of the iron oxide prepared in Example 1 of the present invention;

[0025] Figure 5 is a scanning electron image of the iron oxide prepared in Example 2 of the present invention;

[0026] Figure 6 is a scanning electron image of the iron oxide prepared in Example 3 of the present invention;

[0027] Figure 7 is a scanning electron image of the iron oxyhydroxide prepared in Comparative Example 1 of the present invention;

[0028] Figure 8 is a scanning electron image of the iron oxyhydroxide prepared in Comparative Example 2 of the present invention;

[0029] Fig. 9 is the XRD of the synthetic products of Examples 1, 2, 3 and Comparative Examples 1 and 2,

[0030] Among them, (a) Example 1, (b) Example 2, (c) Example 3, (d) Comparative Example 1, and (e) Comparative Example 2. DETAILED DESCRIPTION

[0031] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.

[0032] The present invention provides a method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite, comprising the following steps: (1) adding ferric nitrate nonahydrate to deionized water, and then cooling to room temperature after reacting for a period of time under constant temperature water bath stirring; collecting the precipitate by centrifugation, and repeatedly washing with deionized water, and finally freeze drying to obtain ferrihydrite powder; dispersing the ferrihydrite powder into an aqueous solution to obtain a ferrihydrite solution. The concentration of ferric nitrate nonahydrate in the deionized solution is 8-10 g / L, the concentration of ferrihydrite in the ferrihydrite solution is 5-10 mg / mL, the constant temperature water bath temperature is 65-75°C, the stirring time is 10-12 min, the centrifugal speed is 15000-17000 rpm, the centrifugal time is 10-20 min, the number of deionized water washings is three times, and the freeze drying time is 24 h. (2) adding ferric chloride and urea to deionized water, and continuously stirring to obtain a mineralized solution. Add the ferrihydrite solution dropwise under continuous stirring, and continue stirring to obtain a mixed mineralized solution containing ferrihydrite. The reactor containing the mixed mineralization solution is placed in a constant temperature oven for full reaction and then cooled naturally to room temperature. The precipitate is collected by centrifugation, repeatedly washed with deionized water, and finally freeze-dried to obtain an iron oxide mesoscopic crystal product. Among them, the concentration of ferric chloride in the mineralization solution is 0.8-1.2M / L, the concentration of urea is 0.8-1.2M / L, the concentration of ferrihydrite in the mixed mineralization solution is 200-600μg / mL, the stirring time is 10-12min, the oven temperature is 60-100℃, the reaction time is 24-96h, the centrifugal speed is 8000-9000rpm, the centrifugal time is 10-20min, the number of deionized water washings is three times, and the freeze-drying time is 24h.

[0033] Example 1

[0034] A method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite comprises the following steps:

[0035] (1) Add 2 g of ferric nitrate nonahydrate to 200 mL of deionized solution, and then stir the mixture in a constant temperature water bath at 75° C. for 10 min and cool to room temperature; centrifuge the mixture at a speed of 16,000 rpm for 20 min, wash the mixture three times with deionized water, and freeze-dry the mixture for 24 h to obtain ferrihydrite powder; disperse 10 mg of the ferrihydrite powder in 2 mL of deionized water to obtain a ferrihydrite solution with a concentration of 5 mg / mL;

[0036] (2) Add 0.8125 g of ferric chloride and 0.3 g of urea to 5 mL of deionized water, and continue stirring for 10 minutes to obtain a mineralized solution; add the ferrihydrite solution dropwise under continuous stirring, and continue stirring for 20 minutes to obtain a mixed mineralized solution containing 300 μg / mL ferrihydrite; place the reactor containing the mixed mineralized solution in an oven at a temperature of 60°C, react for 96 hours, and then naturally cool to room temperature; centrifuge at a speed of 9000 rpm for 10 minutes, then repeatedly wash with deionized water three times, and freeze-dry for 24 hours to obtain an iron oxide mesoscopic crystal product.

[0037] like Figure 1 As shown in the figure, the structure of ferrihydrite was analyzed by transmission electron microscopy. The results showed that the synthesized ferrihydrite had a uniform particle size of about 25 nm. The mineralization product was detected by XRD and scanning electron imaging. The XRD results are shown in Fig. 9 As shown in the curve a, the results show that the product synthesized under the guidance of ferrihydrite at 70°C is a single iron oxide phase. Figure 2 As shown in the scanning electron image results, the results show that the synthesized iron oxide is a nanoparticle with a uniform particle size of about 150nm. Figure 3 As shown in the figure, the microstructure of iron oxide is observed by transmission electron microscopy. Iron oxide is assembled from nanoparticles. The electron diffraction of a single particle is a single crystal diffraction spot, and the diffraction point has a little tail, which is a typical mesoscopic crystal feature. Figure 4 As shown in the figure, the cycle performance of the iron oxide mesoscopic crystal of this embodiment 1 as the negative electrode of the lithium battery is 200mA g -1 After 100 cycles at a current density of 1.5 Å, the capacity is still maintained at 804.5 mA hg -1 , has good lithium battery performance, indicating that the iron oxide has potential application value in energy materials.

[0038] Example 2

[0039] A method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite comprises the following steps:

[0040] (1) Add 1.8 g of ferric nitrate nonahydrate to 200 mL of deionized solution, and then stir the mixture in a 70°C constant temperature water bath for 10 min and cool to room temperature. Centrifuge for 20 min at a speed of 16,000 rpm, wash three times with deionized water, and freeze-dry for 24 h to obtain ferrihydrite powder. Disperse 10 mg of ferrihydrite powder in 1 mL of deionized water solution to obtain a ferrihydrite solution with a concentration of 10 mg / mL.

[0041] (2) Add 0.79 g of ferric chloride and 0.285 g of urea to 5 mL of deionized water, and continue stirring for 10 minutes to obtain a mineralized solution. Add the ferrihydrite solution dropwise while continuing to stir, and continue stirring for 20 minutes to obtain a mixed mineralized solution containing 200 μg / mL ferrihydrite. Place the reactor containing the mixed mineralized solution in an oven at 80°C, react for 48 hours, and then cool naturally to room temperature. Centrifuge at a speed of 9000 rpm for 10 minutes, then wash repeatedly with deionized water three times, and freeze-dry for 24 hours to obtain an iron oxide mesoscopic crystal product.

[0042] The mineralization products were detected by XRD and scanning electron imaging. The XRD results are as follows: Fig. 9 As shown in the curve b, the results show that the product synthesized under the guidance of ferrihydrite at 80°C is a single iron oxide phase. Figure 5 As shown, the scanning electron image results show that the synthesized iron oxide is a nanoparticle with a uniform particle size of about 300nm.

[0043] Example 3

[0044] A method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite comprises the following steps:

[0045] (1) Add 1.9 g of ferric nitrate nonahydrate to 200 mL of deionized solution, and then stir the mixture in a constant temperature water bath at 65°C for 12 min and cool to room temperature. Centrifuge for 20 min at a speed of 16,000 rpm, wash three times with deionized water, and freeze-dry for 24 h to obtain ferrihydrite powder. Disperse 10 mg of ferrihydrite powder in 2 mL of deionized water to obtain a ferrihydrite solution with a concentration of 5 mg / mL.

[0046] (2) Add 0.805 g of ferric chloride and 0.306 g of urea to 5 mL of deionized water and continue stirring for 10 min to obtain a mineralized solution. Add the ferrihydrite solution dropwise while continuing to stir, and continue stirring for 20 min to obtain a mixed mineralized solution containing 600 μg / mL ferrihydrite. Place the reactor containing the mixed mineralized solution in an oven at 100°C, react for 24 hours, and then cool naturally to room temperature. Centrifuge at 9000 rpm for 10 minutes, then wash repeatedly with deionized water three times, and freeze-dry for 24 hours to obtain an iron oxide mesoscopic crystal product.

[0047] The mineralization products were detected by XRD and scanning electron imaging. The XRD results are as follows: Fig. 9 As shown in the curve c, the results show that the product synthesized under the guidance of ferrihydrite at 100°C is a single iron oxide phase. Figure 6 As shown, the scanning electron image results show that the synthesized iron oxide nanoparticles have a particle size of about 200 to 500 nm.

[0048] Comparative Example 1

[0049] The hydrothermal synthesis of iron oxyhydroxide guided by pure water includes the following steps:

[0050] Weigh 0.8125g of ferric chloride and 0.3g of urea into a beaker, add 5mL of deionized water, and stir for 10 minutes to obtain a mineralization solution. Place the reactor containing the above solution in an oven at 70°C, react for 96 hours, and then cool naturally to room temperature. Centrifuge for 10 minutes at a speed of 9000rpm, wash three times with deionized water, and freeze-dry for 24 hours to obtain a hydroxyl iron powder product.

[0051] The mineralization products were detected by XRD and scanning electron imaging. The XRD results are as follows: Fig. 9 As shown in the curve d in the middle, the results show that the product synthesized with pure water at 70°C is a single oxyhydroxide iron phase. The results of the comparative experiment with pure water show that iron oxide cannot be synthesized at a lower temperature of 70°C. The scanning electron image results are shown in Figure 7 As shown, the results show that the synthesized iron oxyhydroxide is a nanorod with a diameter of about 100 nm.

[0052] Comparative Example 2

[0053] The hydrothermal synthesis of iron oxyhydroxide guided by pure water includes the following steps:

[0054] Weigh 0.805g of ferric chloride and 0.31g of urea into a beaker, add 5mL of deionized water, and stir for 10 minutes to obtain a mineralization solution. Place the reactor containing the above solution in an oven at 100°C, react for 48 hours, and then cool to room temperature naturally. Centrifuge for 10 minutes at a speed of 9000rpm, wash three times with deionized water, and freeze-dry for 24 hours to obtain a ferric hydroxide powder product.

[0055] The mineralization products were detected by XRD and scanning electron imaging. The XRD results are as follows: Fig. 9 As shown in the curve e, the results show that the product synthesized with pure water at 100°C is a single oxyhydroxide iron phase. The results of the comparative experiment with pure water show that iron oxide cannot be synthesized at a lower temperature of 100°C. The scanning electron image results are shown in Figure 8 As shown, the results show that the synthesized iron oxyhydroxide is a nanorod with a diameter of about 100nm. Based on the above experimental results, iron oxide mesoscopic crystals were synthesized by mineralization of ferrihydrite at near room temperature.

[0056] In summary, the embodiments of the present invention show that the use of ferrihydrite modifiers can synthesize iron oxide mesoscopic crystals at near room temperature, the preparation conditions are simple, and the particle size of the mineralized product is uniform, while in the comparative example where the ferrihydrite modifier is not used, iron oxide cannot be synthesized at near room temperature. The present invention provides an innovative preparation method for the low-temperature, low-energy synthesis of iron oxide materials.

[0057] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite, characterized in that: The following steps are involved: S1. Adding ferric nitrate nonahydrate to deionized water, and then reacting for a period of time in a constant temperature water bath with stirring, and then cooling to room temperature; collecting the precipitate by centrifugation, and repeatedly washing it with deionized water, and finally freeze-drying it to obtain ferrihydrite powder; dispersing the ferrihydrite powder into an aqueous solution to obtain a ferrihydrite solution; S2. Add ferric chloride and urea to deionized water, and continue stirring to obtain a mineralized solution; add ferrihydrite solution dropwise under continuous stirring, and continue stirring to obtain a mixed mineralized solution containing ferrihydrite; place the reactor containing the mixed mineralized solution in a constant temperature oven for sufficient reaction and then naturally cool to room temperature; collect the precipitate by centrifugation, wash it repeatedly with deionized water, and finally freeze-dry it to obtain an iron oxide mesoscopic crystal product.

2. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 1, characterized in that: In the step S1, the concentration of ferric nitrate nonahydrate in the deionized solution is 8-10 g / L. The concentration of ferrihydrite in the ferrihydrite solution is 5-10 mg / mL.

3. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 2, characterized in that: In step S1, the temperature of the constant temperature water bath is 65-75° C., and the stirring time is 10-12 min.

4. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 3, characterized in that: In the step S1, the centrifugal speed is 15000-17000 rpm, the centrifugal time is 10-20 min, the number of deionized water washing is three times, and the freeze-drying time is 24 h.

5. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 1, characterized in that: The concentration of ferric chloride in the mineralization solution is 0.8-1.2 M / L, the concentration of urea is 0.8-1.2 M / L, and the concentration of ferrihydrite in the mixed mineralization solution is 200-600 μg / mL.

6. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 5, characterized in that: In step S2, the stirring time is 10 to 12 minutes.

7. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 6, characterized in that: In step S2, the oven temperature is 60-100° C., and the reaction time is 24-96 hours.

8. The method for synthesizing iron oxide mesoscopic crystals by low-temperature mineralization of ferrihydrite according to claim 7, characterized in that: In the step S2, the centrifugal speed is 8000-9000 rpm, the centrifugal time is 10-20 min, the number of deionized water washing is three times, and the freeze-drying time is 24 h.

Citation Information

Patent Citations

  • Method of preparing monodisperse iron oxide quasi-cubic mesoscopic crystal with adjustable grain size

    CN103482708A