High-brightness lithium disilicate glass ceramic, preparation method thereof and obtained product

By controlling the basic glass components and additives of lithium disilicate glass ceramics, and optimizing the process, the problems of low brightness and easy to gray in the existing technology are solved, high brightness and good light transmission performance are achieved, and the scope of use is broadened. 和美学效果。

CN118930058AInactive Publication Date: 2024-11-12SHENZHEN UPCERA DENTAL TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411150002.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium disilicate glass ceramics have low brightness in the field of dental restoration, which leads to limited use range. The frequent external dyeing times can easily lead to gray color, making it difficult to achieve ideal results.

Method used

By controlling the molar percentage range of the base glass components and the combination of additives, high-quality lithium disilicate glass ceramics are prepared, including improving brightness while maintaining the transparency and optimizing through melting and forming processes to achieve Refine grains and high refractive index to enhance light transmission performance.

Benefits of technology

With the transparency remains unchanged, the brightness of lithium disilicate glass ceramics is significantly improved, the scope of use is broadened, the number of external dyeing is reduced, the color is grayed out, and the demand for high-quality restorations is maintained. Good aesthetic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003378720000011
    Figure BDA0005003378720000011
  • Figure BDA0005003378720000021
    Figure BDA0005003378720000021
  • Figure BDA0005003378720000022
    Figure BDA0005003378720000022
Patent Text Reader

Abstract

The invention provides a high-brightness lithium disilicate glass ceramic, a preparation method thereof and an obtained product, and belongs to the technical field of lithium disilicate glass ceramics. The high-brightness lithium disilicate glass ceramic provided by the invention at least comprises a basic glass component, and the molar percentages of the components in the basic glass component meet the following ranges: 0.4 < = (Li2O + P2O5) / (SiO2 + Al2O3) < = 0.55, 0.05 < = P2O5 / Li2O < = 0.1. The high-brightness lithium disilicate glass ceramic provided by the invention has higher brightness and better aesthetic effect under the condition that the transparency is kept unchanged, and is more beneficial to technician end operation such as external dyeing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium disilicate glass ceramics, and in particular relates to high-brightness lithium disilicate glass ceramics, a preparation method thereof and the obtained product. Background Art

[0002] In the field of dental clinical restoration, lithium disilicate glass ceramics occupy a certain market share, largely due to its good aesthetic effect, but most restorations made from lithium disilicate glass ceramic blocks have low brightness, which limits its scope of use. In addition, many restorations need to be dyed externally to achieve a color close to the patient's tooth color, but in many cases, one external dyeing cannot achieve the desired effect. If the technician is not very skilled, more external dyeing is required to achieve the desired effect. As we all know, the more times the external dyeing is done, the more likely the restoration is to be gray, causing the color of the restoration to deviate from the desired effect, but the gray brightness after external dyeing cannot be solved. Therefore, there is an urgent need for a lithium disilicate glass ceramic that can have a higher brightness while maintaining the same transparency. Summary of the invention

[0003] The present invention provides a high-brightness lithium disilicate glass ceramic, a preparation method thereof and the resulting product, which can maintain the same transparency while having a higher-brightness lithium disilicate glass ceramic, a better aesthetic effect, and is more conducive to technical operations such as external dyeing.

[0004] In order to achieve the above object, the present invention provides a high-brightness lithium disilicate glass ceramic, which comprises at least a basic glass component, wherein the molar percentages of the components in the basic glass component satisfy the following ranges:

[0005] 0.4≤(Li2O+P2O5) / (SiO2+Al2O3)≤0.55

[0006] 0.05≤P2O5 / Li2O≤0.1.

[0007] Preferably, the basic glass component includes the following components in percentage by mass:

[0008]

[0009]

[0010] Preferably, the basic glass component includes the following components in percentage by mass:

[0011]

[0012] Preferably, the basic glass component further comprises a compound containing Tb ions, and its content is 0.2-0.5%, preferably 0.3-0.4%, calculated as a percentage by mass of Tb4O7.

[0013] Preferably, the additive is further included, wherein the additive is selected from at least one of alkaline earth metal oxides, trivalent element oxides, tetravalent element oxides, pentavalent element oxides and hexavalent element oxides, and the content of the additive is 0-12wt%;

[0014] The alkaline earth metal oxide is selected from at least one of CaO, BaO, MgO, SrO or a mixture thereof; the oxide of the trivalent element is other than Al2O3 and is selected from at least one of B2O3, Y2O3, La2O3, Bi2O3 or a mixture thereof; the oxide of the tetravalent element is other than SiO2, ZrO2, TiO2 and is selected from at least one of SnO2, TiO2 and GeO2; the oxide of the pentavalent element is selected from at least one of P2O5 and Nb2O5; the oxide of the hexavalent element is selected from at least one of WO3 and MoO3.

[0015] Preferably, it further comprises a colorant, wherein the colorant is selected from at least one of a yellow colorant, a red colorant, and a gray colorant, and the content thereof is 0-5.5wt%, preferably 0.5-3.5%;

[0016] The yellow colorant is selected from at least one of CeO2, Pr2O3, and V2O5; the red colorant is Er2O3; and the gray colorant is selected from at least one of MnO, NiO, and Nd2O3.

[0017] Preferably, it further comprises a fluorescent agent, wherein the fluorescent agent comprises at least one of oxides, carbonates, nitrates and phosphates of at least two of the following elements Sm, Dy, Er, Yb, Nd, Tm and Eu, and the content thereof is 0.1-3 wt%, preferably 0.2-1.5% wt%;

[0018] The base glass component also includes no more than 0.01 wt % of Fe ions.

[0019] The present invention also provides a method for preparing the high-brightness lithium disilicate glass ceramic according to any one of the above technical solutions, comprising the following steps:

[0020] According to the formula, basic glass components, additives, colorants and fluorescent agents are selected and mixed evenly, melted and water quenched in an air atmosphere, the quenched glass frit is melted again, and the melted glass liquid is poured into the required mold for molding and heat treatment.

[0021] Preferably, the melting temperature is 1450°C-1650°C, and the holding time is 60-120min;

[0022] The remelting temperature is 1450℃-1650℃, and the holding time is 60-120min;

[0023] The heat treatment temperature is 500-1100°C, preferably 600-1000°C.

[0024] The present invention also provides a method for preparing the high-brightness lithium disilicate glass ceramic according to any one of the above technical solutions, comprising the following steps:

[0025] According to the formula, basic glass components, additives, colorants and fluorescent agents are selected and mixed evenly, and melted in an air atmosphere. After melting, the glass liquid is homogenized and then poured into cold water to obtain a glass frit. The obtained glass frit is polished to obtain glass powder, and the obtained glass powder is placed in a required mold for dry pressing and isostatic pressing, and then sintered in a vacuum atmosphere.

[0026] Preferably, the melting temperature is 1350°C-1550°C, and the holding time is 30-60min;

[0027] The molding pressure of dry pressing is 10-20MPa, and the pressure of isostatic pressing is 200-300MPa;

[0028] The sintering temperature is 700-1000°C, and the vacuum degree is controlled below 1000-4000Pa.

[0029] The present invention also provides a dental restoration prepared by using the high-brightness lithium disilicate glass ceramics according to any one of the above technical solutions.

[0030] Preferably, compared with the traditional lithium disilicate glass ceramics, it can have a brightness that is 2-4 higher than the traditional lithium disilicate glass ceramics while maintaining similar color and unchanged transparency.

[0031] Preferably, the dental restoration is prepared by adopting a CAD / CAM process or a hot die casting process.

[0032] Compared with the prior art, the advantages and positive effects of the present invention are:

[0033] 1. The present invention defines the scope of the entire formula by controlling the relationship between components. The formula within this specific range can be used through a series of processes to produce lithium disilicate glass ceramics with higher brightness while maintaining the same transparency.

[0034] 2. Different from traditional glass ceramics, the internal structure of the lithium disilicate glass ceramics provided by the present application has finer grains, and the refined grain size is more uniform, with a higher refractive index and better light transmittance. This leaves more room for increasing brightness and reducing transmittance. Therefore, when the brightness of the formula is increased by adjusting, the originally increased transmittance makes up for the decrease in transmittance caused by the increase in brightness, so that the glass ceramics can have a higher brightness while keeping the transmittance unchanged.

[0035] 3. The present invention can have lithium disilicate glass ceramics with higher brightness while maintaining the same transparency, which greatly broadens its scope of use, provides technicians with more operating space, improves customer experience, and fundamentally solves the problem of graying of restorations due to external staining. It can also meet the needs of high-brightness restorations while maintaining good transparency and ensuring aesthetic effects. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1 (Melting Method CAD Secondary Crystallization)

[0038] According to the component contents shown in Table 1 below, the raw material components of the basic glass are prepared, and each raw material can be selected from its oxide, carbonate or phosphate, etc., and mixed thoroughly; the mixed raw materials are put into a platinum crucible, and the platinum crucible is put into a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1550°C and the melting time is 60 minutes to homogenize the glass liquid, and then poured into cold water to obtain a glass block; the glass block is melted at 1550°C for 60 minutes, and then cast into a mold for molding, and the ceramic block is crystallized at 600°C in a box furnace to obtain a CAD ceramic block.

[0039] The obtained CAD ceramic block is processed through CAD / CAM process and crystallized at 900°C to prepare lithium disilicate glass-ceramic restorations.

[0040] Table 1

[0041] Element Content wt% SiO2 68.5 Li2O 13.2 ZnO 3.7 K2O 3 Al2O3 2.34 ZrO2 1.3 P2O5 5.6 Tb4O7 1 V2O5 0.06 Er2O3 0.2 Tm2O3 0.4 Eu2O3 0.7

[0042] Conventional HTBL2 is a representative lithium disilicate glass ceramic product, and therefore as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of Example 1.

[0043] Sample name L a b Transmittance Traditional HTBL2 76.93 -0.78 2.38 42.82 Example 1 79.85 -0.62 2.11 42.36

[0044] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 1 of the present invention is higher, with a higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0045] Example 2 (Melting CAD Secondary Crystallization)

[0046] According to the component contents shown in Table 2 below, the raw material components of the basic glass are prepared, and each raw material can be selected from its oxide, carbonate or phosphate, etc., and mixed thoroughly; the mixed raw materials are put into a platinum crucible, and the platinum crucible is put into a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1500°C and the melting time is 90 minutes to homogenize the glass liquid, and then poured into cold water to obtain a glass block; the glass block is then melted at 1450°C for 90 minutes, and then cast into a mold for molding, and the ceramic block is crystallized at 650°C in a box furnace to obtain a CAD ceramic block.

[0047] The obtained CAD ceramic block is processed through CAD / CAM process and crystallized at 950°C to prepare lithium disilicate glass-ceramic restorations.

[0048] Table 2

[0049] Element Content wt% SiO2 71.3 Li2O 14.7 P2O5 3.5 K2O 4.4 Al2O3 1.6 ZrO2 0.7 ZnO 0.3 Tb4O7 0.5 BaO 0.4 MgO 0.1 La2O3 0.2 TiO2 0.2 Er2O3 0.1 CeO2 1.5 MnO 0.05 Tm2O3 0.15 Eu2O3 0.3

[0050] Conventional LTBL2 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0051] Sample name L a b Transmittance Traditional LTBL2 80.65 -0.57 3.34 39.09 Example 2 83.47 -0.72 2.89 38.48

[0052] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 2 of the present invention is higher, with a higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0053] Example 3 (Melting CAD Secondary Crystallization)

[0054] According to the component contents shown in Table 3 below, the raw material components of the basic glass are prepared, and each raw material can be selected as its oxide, carbonate or phosphate, etc., and mixed thoroughly; the mixed raw materials are put into a platinum crucible, and the platinum crucible is placed in a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1530°C and the melting time is 70 minutes to homogenize the glass liquid, and then poured into cold water to obtain a glass block; the glass block is melted at 1530°C for 70 minutes, and then cast into a mold to form, and the ceramic block is crystallized at 670°C in a box furnace to obtain a CAD ceramic block.

[0055] The obtained CAD ceramic block is processed through CAD / CAM process and crystallized at 930°C to prepare lithium disilicate glass-ceramic restoration.

[0056] Table 3

[0057]

[0058]

[0059] Conventional LTA2 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0060] Sample name L a b Transmittance Traditional LTA2 71.25 1.18 14.11 37.53 Example 3 74.08 1.27 13.84 37.62

[0061] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 3 of the present invention is higher, with higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0062] Example 4 (Melting Method CAD Secondary Crystallization)

[0063] According to the component contents shown in Table 4 below, the raw material components of the basic glass are prepared, and each raw material can be selected as its oxide, carbonate or phosphate, etc., and mixed thoroughly; the mixed raw materials are put into a platinum crucible, and the platinum crucible is placed in a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1600°C and the melting time is 60 minutes to homogenize the glass liquid, and then poured into cold water to obtain a glass frit; the glass frit is then melted at 1600°C for 60 minutes, and then cast into a mold to form, and the ceramic block is crystallized at 630°C in a box furnace to obtain a CAD ceramic block.

[0064] The obtained CAD ceramic block is processed through CAD / CAM process and crystallized at 860°C to prepare lithium disilicate glass-ceramic restoration.

[0065] Table 4

[0066] Element Content wt% SiO2 68.9 Li2O 14.3 P2O5 3.9 K2O 4.7 Al2O3 4.4 ZrO2 2 ZnO 0.2 Tb4O7 0.2 CaO 0.1 MgO 0.3 MoO3 0.5 V2O5 0.2 Nd2O3 0.1 Eu2O3 0.2

[0067] Conventional HTA2 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0068] Sample name L a b Transmittance Traditional HTA2 68.48 0.10 11.68 43.46 Example 4 71.63 0.02 11.88 43.18

[0069] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 4 of the present invention is higher, with higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0070] Example 5 (melting press)

[0071] According to the component contents shown in Table 5 below, prepare the raw material components of the basic glass, and each raw material may be selected as its oxide, carbonate or phosphate, etc., and mix them thoroughly and evenly; put the mixed raw materials into a platinum crucible, put the platinum crucible into a furnace under an air atmosphere for melting, control the melting temperature to 1550°C, and the melting time to 80 minutes, so that the glass liquid is homogenized, and then poured into cold water to obtain a glass frit; the glass frit is then melted at 1550°C for 60 minutes, and then cast into a mold to form, and the porcelain block is crystallized at 880°C in a box furnace to obtain a press porcelain block.

[0072] The obtained press ceramic block can be used to prepare a lithium disilicate glass ceramic restoration through a hot pressure casting process.

[0073] Table 5

[0074] Element Content wt% SiO2 65.4 Li2O 12 ZnO 4.7 K2O 4.5 Al2O3 1.2 ZrO2 3.3 P2O5 5.7 CaO 1 MgO 0.5 La2O3 0.41 Tb4O7 1 V2O5 0.16 Er2O3 0.2 Tm2O3 0.4 Eu2O3 0.7

[0075] Conventional HTBL1 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0076] Sample name L a b Transmittance Traditional HTBL1 78.71 -0.68 -0.63 44.38 Example 5 81.35 -0.62 -0.21 44.16

[0077] In the table, the L value represents the lightness value, the larger the L value, the higher the lightness, the a value represents the red value, the larger the a value, the more red, the b value represents the yellow value, the larger the b value, the more yellow, the lightness of the product is closely related to the color and transmittance, the darker the color, the lower the transmittance, and the lower the lightness, but when the color is fixed, the higher the lightness, the lower the transmittance, and the higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close, and when the transmittance is close, the L value of the sample in Example 5 of the present invention is higher, with higher lightness, and a value of about 3 higher. Generally, external dyeing will cause the lightness value to drop by about 1-3, so the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0078] Example 6 (melting press)

[0079] According to the component contents shown in Table 6 below, the raw material components of the basic glass are prepared, and each raw material can be selected from its oxide, carbonate or phosphate, etc., and mixed thoroughly; the mixed raw materials are put into a platinum crucible, and the platinum crucible is placed in a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1600°C and the melting time is 60 minutes to homogenize the glass liquid, and then poured into cold water to obtain a glass frit; the glass frit is then melted at 1600°C for 60 minutes, and then cast into a mold to form, and the porcelain block is crystallized at 900°C in a box furnace to obtain a press porcelain block.

[0080] The obtained press ceramic block can be used to prepare a lithium disilicate glass ceramic restoration through a hot pressure casting process.

[0081] Table 6

[0082]

[0083]

[0084] Conventional LTBL3 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0085] Sample name L a b Transmittance Traditional LTBL3 78.28 -0.03 5.98 38.78 Example 6 81.47 -0.12 6.29 38.48

[0086] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 6 of the present invention is higher, with higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0087] Example 7 (melting press)

[0088] According to the component contents shown in Table 7 below, prepare the raw material components of the basic glass, and each raw material may be selected as its oxide, carbonate or phosphate, etc., and mix them thoroughly; put the mixed raw materials into a platinum crucible, put the platinum crucible into a furnace under an air atmosphere for melting, control the melting temperature to 1550°C, and the melting time to 80 min, so that the glass liquid is homogenized, and then poured into cold water to obtain a glass frit; the glass frit is then melted at 1550°C for 80 min, and then cast into a mold to form, and the porcelain block is crystallized at 850°C in a box furnace to obtain a press porcelain block.

[0089] The obtained press ceramic block can be used to prepare a lithium disilicate glass ceramic restoration through a hot pressure casting process.

[0090] Table 7

[0091]

[0092]

[0093] Conventional LTA1 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0094] Sample name L a b Transmittance Traditional LTA1 74.35 0.13 12.64 36.67 Example 7 77.08 0.27 11.84 35.42

[0095] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 7 of the present invention is higher, with a higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0096] Example 8 (melting press)

[0097] According to the component contents shown in Table 8 below, prepare the raw material components of the basic glass, and each raw material may be selected as its oxide, carbonate or phosphate, etc., and mix them thoroughly and evenly; put the mixed raw materials into a platinum crucible, put the platinum crucible into a furnace under an air atmosphere for melting, control the melting temperature to 1450°C, and the melting time to 120 min, so that the glass liquid is homogenized, and then poured into cold water to obtain a glass frit; the glass frit is then melted at 1450°C for 120 min, and then cast into a mold to form, and the ceramic block is crystallized at 880°C in a box furnace to obtain a press ceramic block.

[0098] The obtained press ceramic block can be used to prepare a lithium disilicate glass ceramic restoration through a hot pressure casting process.

[0099] Table 8

[0100] Element Content wt% SiO2 68.1 Li2O 13.9 P2O5 4.5 K2O 4.7 Al2O3 3.6 ZrO2 2.2 ZnO 0.2 Tb4O7 0.2 CaO 0.6 MgO 0.5 MoO3 0.5 V2O5 0.4 Nd2O3 0.1 Eu2O3 0.5

[0101] Conventional HTA3 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0102] Sample name L a b Transmittance Traditional HTA3 66.9 0.43 12.78 43.05 Example 8 70.63 0.22 11.94 42.33

[0103] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 8 of the present invention is higher, with a higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0104] Example 9 (Sintering CAD Secondary Crystallization)

[0105] According to the component contents shown in Table 9 below, the raw material components of the basic glass are prepared, and each raw material can be selected from its oxide, carbonate or phosphate, etc., and mixed thoroughly; the mixed raw materials are put into a platinum crucible, and the platinum crucible is placed in a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1400°C, and the melting time is 60min, so that the glass liquid is homogenized, and then poured into cold water to obtain a glass frit; the frit is coarsely ground and finely ground to a particle size of D50=2μm, and the ground glass powder is placed in a prepared mold, dry pressed at a molding pressure of 20MPa, and then isostatically pressed at a pressure of 240MPa; the green blank is sintered in a vacuum atmosphere furnace at a temperature of 650°C and a vacuum degree controlled at 2600Pa.

[0106] The obtained CAD ceramic block can be prepared into a blank through the CAD / CAM process, and then subjected to a crystallization treatment at 880°C to obtain a lithium disilicate glass-ceramic restoration.

[0107] Table 9

[0108]

[0109]

[0110] Conventional LTA3 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0111] Sample name L a b Transmittance Traditional LTA3 67.85 2.26 16.63 36.69 Example 9 71.08 2.07 16.84 35.62

[0112] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 9 of the present invention is higher, with higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

[0113] Example 10 (Sintering Press)

[0114] According to the component contents shown in Table 10 below, the raw material components of the basic glass are prepared, and each raw material can be selected from its oxide, carbonate or phosphate, etc., and are fully mixed; the mixed raw materials are put into a platinum crucible, and the platinum crucible is placed in a furnace for melting under an air atmosphere, and the melting temperature is controlled to be 1450°C and the melting time is 45min to homogenize the glass liquid, and then poured into cold water to obtain a glass frit; the frit is coarsely ground and finely ground to a particle size of D50=5μm, and the ground glass powder is placed in a prepared mold, dry pressed at a molding pressure of 15MPa, and then isostatically pressed at a pressure of 260MPa; the green blank is sintered in a vacuum atmosphere furnace at a temperature of 860°C and a vacuum degree controlled at 3000Pa.

[0115] The obtained press ceramic block can be used to prepare a lithium disilicate glass ceramic restoration through a hot pressure casting process.

[0116] Table 10

[0117]

[0118]

[0119] Conventional HTA1 is a representative lithium disilicate glass ceramic product, so as a comparative example, the following is a comparison of its tested color and transmittance values ​​with those of the embodiment.

[0120] Sample name L a b Transmittance Traditional HTA1 70.12 -0.09 9.23 43.91 Example 10 73.63 0.02 9.88 43.15

[0121] In the table, the L value represents the lightness value. The larger the L value, the higher the lightness. The a value represents the red value. The larger the a value, the more red. The b value represents the yellow value. The larger the b value, the more yellow. The lightness of the product is closely related to the color and transmittance. The darker the color, the lower the transmittance and the lower the lightness. However, when the color is fixed, the higher the lightness, the lower the transmittance. The higher the transmittance, the lower the lightness. As can be seen from the above table, the color a value and b value of the two samples are close. When the transmittance is close, the L value of the sample in Example 10 of the present invention is higher, with higher lightness, which is about 3 higher. Generally, external dyeing will reduce the lightness value by about 1-3. In this way, the higher lightness of the present invention can completely make up for the influence of external dyeing on the reduction of lightness value.

Claims

1. A high brightness lithium disilicate glass ceramic, characterized in that: At least a basic glass component is included, and the molar percentages of the components in the basic glass component meet the following ranges: 0.4≤(Li2O+P2O5) / (SiO2+Al2O3)≤0.55 0.05≤P2O5 / Li2O≤0.

1.

2. The high-brightness lithium disilicate glass ceramic according to claim 1, characterized in that: The basic glass component includes the following components in percentage by mass:

3. The high-brightness lithium disilicate glass ceramic according to claim 2, characterized in that: The basic glass component also includes a compound containing Tb ions, and the content of the compound is 0.2-0.5% by mass percentage of Tb4O7.

4. The high-brightness lithium disilicate glass ceramic according to claim 2, characterized in that: The invention also includes an additive, wherein the additive is selected from at least one of alkaline earth metal oxides, trivalent element oxides, tetravalent element oxides, pentavalent element oxides and hexavalent element oxides, and the content of the additive is 0-12 wt %; The alkaline earth metal oxide is selected from at least one of CaO, BaO, MgO, SrO or a mixture thereof; the oxide of the trivalent element is other than Al2O3 and is selected from at least one of B2O3, Y2O3, La2O3, Bi2O3 or a mixture thereof; the oxide of the tetravalent element is other than SiO2, ZrO2, TiO2 and is selected from at least one of SnO2, TiO2 and GeO2; the oxide of the pentavalent element is selected from at least one of P2O5 and Nb2O5; the oxide of the hexavalent element is selected from at least one of WO3 and MoO3.

5. The high-brightness lithium disilicate glass ceramic according to claim 2, characterized in that: It also includes a colorant, wherein the colorant is selected from at least one of a yellow colorant, a red colorant, and a gray colorant, and the content thereof is 0-5.5wt%; The yellow colorant is selected from at least one of CeO2, Pr2O3, and V2O5; the red colorant is Er2O3; and the gray colorant is selected from at least one of MnO, NiO, and Nd2O3.

6. The high-brightness lithium disilicate glass ceramic according to claim 2, characterized in that: It also includes a fluorescent agent, wherein the fluorescent agent includes at least one of oxides, carbonates, nitrates, and phosphates of at least two of the following elements Sm, Dy, Er, Yb, Nd, Tm, and Eu, and the content thereof is 0.1-3wt%; The base glass component also includes no more than 0.01 wt % of Fe ions.

7. The method for preparing the high-brightness lithium disilicate glass ceramic according to any one of claims 1 to 6, characterized in that: The following steps are involved: According to the formula, basic glass components, additives, colorants and fluorescent agents are selected and mixed evenly, melted and water quenched in an air atmosphere, the quenched glass frit is melted again, and the melted glass liquid is poured into the required mold for molding and heat treatment.

8. The preparation method according to claim 7, characterized in that: The melting temperature is 1450℃-1650℃, and the holding time is 60-120min; The remelting temperature is 1450℃-1650℃, and the holding time is 60-120min; The heat treatment temperature is 500-1100℃.

9. The method for preparing the high-brightness lithium disilicate glass ceramic according to any one of claims 1 to 6, characterized in that: The following steps are involved: According to the formula, basic glass components, additives, colorants and fluorescent agents are selected and mixed evenly, and melted in an air atmosphere. After melting, the glass liquid is homogenized and then poured into cold water to obtain a glass frit. The obtained glass frit is polished to obtain glass powder, and the obtained glass powder is placed in a required mold for dry pressing and isostatic pressing, and then sintered in a vacuum atmosphere.

10. The preparation method according to claim 9, characterized in that: The melting temperature is 1350℃-1550℃, and the holding time is 30-60min; The molding pressure of dry pressing is 10-20MPa, and the pressure of isostatic pressing is 200-300MPa; The sintering temperature is 700-1000°C and the vacuum degree is controlled at 1000-4000Pa.

11. A dental restoration, characterized in that The high-brightness lithium disilicate glass ceramic is prepared by using the high-brightness lithium disilicate glass ceramic described in any one of claims 1 to 6.

12. The dental restoration according to claim 11, characterized in that Compared with traditional lithium disilicate glass ceramics, it has a brightness that is 2-4 points higher than traditional lithium disilicate glass ceramics while maintaining similar color and unchanged transparency.

Citation Information

Patent Citations

  • Method for producing a dental prosthesis

    CN104955436A

  • Starting glass, lithium silicate glass with core and preparation method and application of lithium silicate glass

    CN112551894A

  • Starting glass, lithium silicate glass with core, preparation method and application thereof

    CN112694253A

  • Dental lithium silicate glass ceramic, preparation method thereof and lithium silicate glass ceramic prosthesis

    CN113264684A

  • Dental lithium silicate glass ceramic, preparation method thereof and lithium silicate glass ceramic prosthesis

    CN113461336A