Glass powder for thin Poly layer fine grid silver paste on back surface of battery and preparation method of glass powder

By optimizing the combination and preparation process of glass powder A and glass powder B, the problem of silver paste etching damaging the thin POLY layer was solved, thus improving the photoelectric conversion efficiency and environmental friendliness of TOPCon crystalline silicon solar cells.

CN118930059APending Publication Date: 2024-11-12FOSHAN HAOYU XINNENG TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411101214.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the back metallization process of existing TOPCon crystalline silicon solar cells, the excessive etching of silver paste can easily damage the thin POLY layer, leading to reduced passivation effect, increased contact resistance, and affecting photoelectric conversion efficiency.

Method used

By combining two types of glass powder, A and B, and optimizing their weight ratio and particle size, the etching performance of the silver paste was controlled. By adjusting the ratio of PbO, TeO2, Li2O and Na2O in glass powder A and the ratio of PbO, TeO2, WO3 and SiO2 in glass powder B, and combining cold rolling and fluidized bed air jet milling technology, uniform glass powder was prepared, which improved the contact and passivation effects.

Benefits of technology

It effectively reduces the corrosion of the POLY layer by silver paste, improves the open circuit voltage and fill factor, enhances photoelectric conversion efficiency, and the production process is environmentally friendly and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004989427630000061
    Figure BDA0004989427630000061
  • Figure BDA0004989427630000071
    Figure BDA0004989427630000071
  • Figure BDA0004989427630000072
    Figure BDA0004989427630000072
Patent Text Reader

Abstract

The invention discloses glass powder for thin Poly layer fine grid silver paste on the back surface of a battery, the glass powder comprises glass powder A and glass powder B, and the weight ratio of the glass powder A to the glass powder B is (1.5-2.5): (0.1-0.5). According to the glass powder for the thin Poly layer and the fine grid silver paste on the back surface of the cell, the contact resistance between the thin Poly layer on the back surface of an N-type TOPCon cell and the fine grid silver paste is comprehensively improved, the corrosion of a POLY layer is reduced, and the damage of a tunneling oxide layer is reduced, so that the open-circuit voltage and filling are improved, and the photoelectric conversion efficiency is further improved. And a double-roller machine is adopted for cold rolling, and fluidized bed airflow is adopted for further crushing, so that the wastewater treatment problem and the discharge problem caused by water quenching and wet ball milling are avoided, and the production process is more environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a glass powder for a thin Poly layer fine grid silver paste on the back of a battery and a preparation method thereof, and relates to CO3C, and in particular to the field of glass powder. Background Art

[0002] TOPCon (Tunnel Oxide Passivated Contact) has high-efficiency photoelectric conversion performance and has attracted widespread attention. TOPCon constructs a tunneling silicon oxide and a doped polysilicon layer (POLY layer) on a silicon substrate. The back passivation contact structure allows the majority carriers to pass through and blocks the minority carriers, which can effectively reduce the surface carrier recombination efficiency and improve the battery performance. However, due to the influence of infrared parasitic absorption, the introduction of the POLY layer will increase the optical loss of the battery, especially in the long-wave range of 800-1200nm. Therefore, reducing the thickness of the POLY layer can reduce the influence of infrared parasitic absorption. This is the back metallization of TOPCon crystalline silicon solar cells. Metallization is a process in which the back silver paste etches through the silicon nitride anti-reflection film layer (SiNx layer) and forms contact with the POLY layer. Balancing the contact and opening voltage is crucial to improving the photoelectric conversion efficiency of TOPCon crystalline silicon solar cells.

[0003] Chinese invention patent CN202310148173.7 discloses a glass powder, preparation method and application for silver paste on the back of N-type crystalline silicon cells. By optimizing the particle size of the glass powder and its amount in the silver paste, the rapid formation of silver microcrystals during the sintering process of the silver paste is promoted, the erosion of the Poly-Si layer is reduced, the contact resistivity and metal composite are balanced to a large extent, and the adhesion of the silver paste layer to the base layer after sintering is increased. However, the problem of easy destruction of the thin POLY layer caused by the excessive corrosion of the silver paste is not solved. Chinese invention patent CN202410059235.1 discloses a glass powder for TOPCon back silver paste and its preparation and application. On the basis of the main components, by adjusting the types and addition amounts of auxiliary components and modifying components, the structural stability of the glass is effectively enhanced, the volume thermal expansion is reduced, and the contact resistance and metal-induced recombination rate between metal and semiconductor are reduced. However, the use of transition metals or rare metals as modifying components has a high production cost. Summary of the invention

[0004] In order to comprehensively improve the contact and passivation effects and enhance the photoelectric conversion efficiency of TOPCon crystalline silicon solar cells, the first aspect of the present invention provides a glass powder for a thin Poly layer fine grid silver paste on the back of a cell, wherein the glass powder comprises glass powder A and glass powder B, and the weight ratio of the glass powder A to the glass powder B is (1.5-2.5): (0.1-0.5).

[0005] As a preferred embodiment, the weight ratio of the glass powder A to the glass powder B is (1.8-2.2): (0.2-0.6).

[0006] As a preferred embodiment, the weight ratio of the glass powder A to the glass powder B is (1.9-2.1): (0.3-0.5).

[0007] As a preferred implementation, the weight ratio of the glass powder A to the glass powder B is 2.1:0.3.

[0008] Glass powder A and glass powder B are used in a weight ratio of (1.9-2.1): (0.3-0.5), which can comprehensively improve the contact and passivation effects, reduce the damage of silver paste to the POLY layer, and at the same time, its own good etching performance can fully etch the SiNx layer, ensure the contact between the glass and the POLY layer, improve the stability of the glass powder, and ensure the passivation effect of the tunneling oxide layer, and the overall efficiency is improved. If the preferred weight ratio is exceeded, the thin POLY layer (60-80nm) will be damaged, the passivation effect will be reduced, the open circuit voltage will be worse, and the overall efficiency will be reduced. If it is lower than the preferred weight ratio, it will cause insufficient etching of SiNx, and weak silver dissolving and precipitation capabilities, resulting in poor contact performance between the silver layer and the silicon substrate, high string resistance, low filling, and low overall efficiency.

[0009] As a preferred embodiment, the particle size D50 of the glass powder A is 1.2-1.8 μm, and the particle size D50 of the glass powder B is 1.2-1.8 μm.

[0010] As a preferred embodiment, the particle size D50 of the glass powder A is 1.2-1.5 μm, and the particle size D50 of the glass powder B is 1.4-1.6 μm.

[0011] As a preferred implementation, the particle size D50 of the glass powder A is 1.3 μm, and the particle size D50 of the glass powder B is 1.5 μm.

[0012] As a preferred embodiment, the raw materials for preparing the glass powder A include: PbO, TeO2, Li2O and Na2O, and the weight ratio of PbO, TeO2, Li2O and Na2O is (30-35): (30-35): (1-3): (1-3).

[0013] As a preferred embodiment, the raw materials for preparing the glass powder A include, by weight percentage: PbO30-35%, TeO2 30-35%, Bi2O3 16-22%, ZnO 1.5-5%, Li2O 1-3%, WO3 2-4%, Na2O 1-3%, and SiO2 6-10%.

[0014] The back metallization of TOPCon crystalline silicon solar cells is a process in which the silver paste on the back side etches through the silicon nitride anti-reflection film layer (SiNx layer) and forms contact with the POLY layer. If the etching property of the silver paste on the back side is weak, it will not be able to effectively etch through the SiNx layer, resulting in poor contact between the silver paste and the POLY layer, increased battery series resistance, and reduced photoelectric conversion efficiency. However, if the etching property of the silver paste on the back side is too strong, it will damage the POLY layer and even the silicon oxide layer, especially for ultra-thin POLY layers, which are more easily damaged. Therefore, how to control the etching performance of the silver paste and balance the contact and opening voltage is crucial to improving the photoelectric conversion efficiency of TOPCon crystalline silicon solar cells. The etching performance of the silver paste is mainly controlled by the glass powder in the silver paste. The applicant has found that the etching effect of the silver paste can be improved by using two glass powders in combination. The weight ratio of PbO, TeO2, Li2O and Na2O in glass powder A is (30-35): (30-35): (1-3): (1-3) to obtain a good gold-semiconductor contact. PbO, TeO2, Li2O and Na2O work together to form sufficient etching, ensuring that the glass can enter the POLY layer through SiNx and form contact with the POLY layer. The excellent silver solubility allows a large amount of nanosilver colloids and silver microcrystals to be present between the silver layer and the POLY layer, which provides a good channel for the tunneling effect of electrons, thereby greatly reducing the contact resistance between the silver layer and the silicon substrate. However, when only a single glass powder is used, the silver paste has strong etching properties, and its strong corrosiveness causes irreversible damage to the thin POLY layer. Even a small amount of larger silver microcrystals will penetrate the POLY layer and damage the silicon oxide layer, resulting in poor open circuit voltage and reduced passivation effect.

[0015] As a preferred embodiment, the raw materials for preparing the glass powder B include: PbO, TeO2, WO3 and SiO2, and the weight ratio of PbO, TeO2, WO3 and SiO2 is (25-30): (15-22): (10-15): (8-15).

[0016] As a preferred embodiment, the raw materials for preparing the glass powder B include, by weight percentage: PbO2 5-30%, TeO2 15-22%, Bi2O3 16-22%, ZnO 2-5%, Li2O 2-4%, WO3 10-15%, Na2O 0.5-1%, SiO2 8-15%, and CuO 1-2%.

[0017] The applicant further found that the weight ratio of PbO, TeO2, WO3 and SiO2 in glass powder B (25-30): (15-22): (10-15): (8-15) can ensure a good passivation effect. The combined bond energy of WO3 and SiO2 is strong, which can improve the stability of the glass, increase the glass transition temperature and softening point, increase the viscosity of the glass, and reduce the fluidity, thereby reducing the damage of the glass to the POLY layer. In addition, the applicant found that the solubility of Ag2O in acidic glass (glass powder B) is greater than that in alkaline glass, which can inhibit the abnormal growth of silver microcrystals to a certain extent, further improve the passivation effect, and ensure that silicon oxide is not destroyed.

[0018] The second aspect of the present invention provides a method for preparing glass powder for thin Poly layer fine grid silver paste on the back of a battery, comprising the following steps:

[0019] S1. Mixing the raw materials for preparing glass powder A and glass powder B respectively, loading them into crucibles respectively, and melting them under heat preservation to obtain glass melt A and glass melt B;

[0020] S2 cold-rolling or water-quenching the glass melt A and the glass melt B respectively to obtain glass slag A and glass slag B;

[0021] S3: pour glass slag A and glass slag B into ball mill jars respectively, add zirconium balls, and grind them coarsely in a planetary ball mill for 0.5-1h;

[0022] S4 is coarsely ground and further pulverized to obtain glass powder A and glass powder B.

[0023] As a preferred implementation, the insulation temperature in step S1 is 1000-1200° C., and the insulation time is 20-60 min.

[0024] As a preferred implementation, the insulation temperature in step S1 is 1000° C. and the insulation time is 30 minutes.

[0025] As a preferred embodiment, the molten glass melt in step S2 is cold rolled on a glass double-roller, which can avoid contamination of the glass by impurity ions compared to water quenching.

[0026] As a preferred embodiment, the further pulverization method in step S4 is selected from one or a combination of mechanical pulverization, air flow pulverization, and impact pulverization.

[0027] As a preferred embodiment, the further pulverization in step S4 is performed by air flow pulverization. The fluidized bed air flow mill can be used for effective classification to obtain glass powder that meets the particle size requirements, has a narrow particle size distribution, and has good dispersibility.

[0028] The third aspect of the present invention provides a fine grid silver paste, the preparation raw materials of which include 2-3 parts by weight of the glass powder, 86-89 parts by weight of silver powder, 5-10 parts by weight of an organic vehicle, and 0.5-1 part by weight of an organic solvent.

[0029] As a preferred embodiment, the organic carrier is selected from one or a combination of alcohol ester dodecanedioate, dimethyl oxalate, diethylene glycol dibutyl ether, ethyl cellulose, and acrylic resin.

[0030] As a preferred embodiment, the organic solvent is selected from one or a combination of terpineol, 12-hydroxyethyl ester, 16-hydroxyethyl ester, butyl carbitol, benzyl alcohol, and triethylene glycol butyl ether.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The glass powder for the fine grid silver paste of the thin Poly layer on the back of the battery of the present invention improves the contact performance of the battery by optimizing the weight ratio of PbO, TeO2, Li2O and Na2O in the glass powder A, optimizes the weight ratio of PbO, TeO2, WO3 and SiO2 in the glass powder B, obtains a better passivation effect, and reasonably matches the glass powder A and the glass powder B to comprehensively improve the contact resistance between the thin Poly layer on the back of the N-type TOPCon battery and the fine grid silver paste, reduces the corrosion of the POLY layer, and reduces the damage of the tunneling oxide layer, thereby improving the open circuit voltage and filling, and further improving the photoelectric conversion efficiency.

[0033] (2) The glass powder for the thin Poly layer fine grid silver paste on the back of the battery described in the present invention is cold-rolled by a double-roll mill and further crushed by fluidized bed airflow to obtain glass powder with uniform particle size distribution and good dispersibility, thereby reducing the content of coarse powder and small powder in the glass powder, thereby improving the sintering density of the silver layer and the wettability of the glass powder, reducing the resistance of the silver layer itself and the contact resistance between the silver layer and the Poly layer, effectively improving the filling of the battery and improving the conversion efficiency of the battery.

[0034] (3) The glass powder used for the thin Poly layer fine grid silver paste on the back of the battery described in the present invention is cold-rolled by a double-roll mill and further crushed by fluidized bed airflow, thereby avoiding the wastewater treatment and emission problems caused by water quenching and wet ball milling, and the production process is more green and environmentally friendly. DETAILED DESCRIPTION

[0035] Example 1

[0036] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery, the glass powder comprising glass powder A and glass powder B, the weight ratio of the glass powder A to the glass powder B is 2.1:0.3.

[0037] The particle size D50 of the glass powder A is 1.3 μm, and the particle size D50 of the glass powder B is 1.5 μm.

[0038] The raw materials for preparing the glass powder A and the glass powder B are shown in Table 1 in terms of weight percentage.

[0039] A method for preparing glass powder for thin Poly layer fine grid silver paste on the back of a battery, comprising the following steps:

[0040] S1. Mixing the raw materials for preparing glass powder A and glass powder B respectively, loading them into crucibles respectively, and melting them under heat preservation to obtain glass melt A and glass melt B;

[0041] S2 cold-rolling or water-quenching the glass melt A and the glass melt B respectively to obtain glass slag A and glass slag B;

[0042] S3: pour glass slag A and glass slag B into ball mill jars respectively, add zirconium balls, and grind them in a planetary ball mill for 0.5 h;

[0043] S4 is coarsely ground and further pulverized to obtain glass powder A and glass powder B.

[0044] In step S1, the holding temperature is 1000° C. and the holding time is 30 minutes.

[0045] The molten glass melt in step S2 is cold rolled on a glass twin-roller.

[0046] The further crushing method in step S4 is to crush the glass powder using a fluidized bed jet mill.

[0047] A fine grid silver paste is prepared by raw materials including 2.4 parts by weight of the glass powder, 89 parts by weight of silver powder, 8 parts by weight of an organic carrier, and 0.6 parts by weight of an organic solvent.

[0048] The organic carrier is dimethyl oxalate; and the organic solvent is alcohol ester dodecanedioate.

[0049] The preparation method of the fine grid silver paste is to mix glass powder, an organic carrier and an organic solvent.

[0050] Example 2

[0051] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery. The specific implementation method is the same as that of Example 1, except that the raw materials for preparing the glass powder A do not contain LiO2.

[0052] Example 3

[0053] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery. The specific implementation method is the same as that of Example 1, except that the raw materials for preparing the glass powder A do not contain Na2O.

[0054] Example 4

[0055] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery. The specific implementation method is the same as that of Example 1, except that the weight ratio of the glass powder A to the glass powder B is 2.0:0.4.

[0056] Example 5

[0057] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery. The specific implementation method is the same as that of Example 1, except that the weight ratio of the glass powder A to the glass powder B is 2.2:0.2.

[0058] Comparative Example 1

[0059] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery. The specific implementation method is the same as that of Example 1, except that the glass powder only contains glass powder A.

[0060] Comparative Example 2

[0061] A glass powder for a thin Poly layer fine grid silver paste on the back of a battery. The specific implementation method is the same as that of Example 1, except that the glass powder only contains glass powder B.

[0062] Comparative Example 3

[0063] A glass powder for thin Poly layer fine grid silver paste on the back of a battery, the specific implementation method is the same as that of Example 1, except that in step S4, the further crushing method is to add alcohol and zirconium balls, then ball mill for 60 minutes, filter and dry, and then pass through a 50-mesh sieve to obtain the glass powder.

[0064] Table 1

[0065]

[0066]

[0067] Performance Testing

[0068] The TOPCON back fine grid silver paste in the embodiment and the comparative example was printed onto a TOPCON crystalline silicon solar cell (POLY layer is 60-80 nm) by screen printing technology, and the final cell was obtained by drying and sintering, with the sintering peak temperature being 720° C. The electrical properties of the cell were tested using a HALM tester, and the results are shown in Table 2.

[0069] Table 2

[0070]

[0071] Results analysis: Comparing Example 1, Example 2, and Example 3, Example 2 is that Li2O is not added to glass powder A, and Example 3 is that Na2O is not added to glass powder A. It can be seen from the results that if Li2O or Na2O is not added to glass powder A, the series resistance will increase, FF will decrease, and the efficiency will deteriorate. This is mainly because not adding Li2O and Na2O will reduce the fluidity of the glass, the silver layer is not sintered densely, and there is a gap between the silver layer and the POLY layer, which leads to an increase in body resistance and contact resistance, which increases the series resistance and reduces the efficiency.

[0072] Comparing Example 1, Example 4, and Example 5, Example 4 reduces the proportion of glass powder A and increases the proportion of glass powder B; Example 5 increases the proportion of glass powder A and reduces the proportion of glass powder B. Glass powder A can bring good contact effect, and glass powder B can bring good passivation effect. However, reducing the content of glass powder A will lead to poor contact, and reducing the content of glass powder B will lead to poor passivation effect, so that the series resistance of Example 4 increases, FF decreases, and efficiency deteriorates, and the opening voltage of Example 5 decreases and the efficiency decreases. Therefore, this also further verifies that the optimal ratio of glass powder A to glass powder B is 2.1:0.3.

[0073] Comparing Example 1, Comparative Example 1 and Comparative Example 2, Comparative Example 1 is to add only glass powder A without glass powder B; Comparative Example 2 is to add only glass powder B without glass powder A. The results show that if only glass powder A is added, the opening voltage will become very poor; if only glass powder B is added, the series resistance will become very high and the FF will be low, both of which will lead to low efficiency.

[0074] Compared with Example 1 and Example 3, the glass powder process S4 of Example 3 adopts a planetary ball mill to obtain the glass powder, which will result in a large amount of coarse powder and small powder in the finished glass powder, uneven particle size distribution, poor glass wettability, loose sintering of the silver layer, low FF, and reduced efficiency.

Claims

1. A glass powder for thin Poly layer fine grid silver paste on the back of a battery, characterized in that: The glass powder includes glass powder A and glass powder B, and the weight ratio of the glass powder A to the glass powder B is (1.5-2.5): (0.1-0.5).

2. The glass powder for thin Poly layer fine grid silver paste on the back of the battery according to claim 1, characterized in that: The particle size D50 of the glass powder A is 1.2-1.8 μm, and the particle size D50 of the glass powder B is 1.2-1.8 μm.

3. The glass powder for thin Poly layer fine grid silver paste on the back of the battery according to claim 1, characterized in that: The raw materials for preparing the glass powder A include: PbO, TeO2, Li2O and Na2O, and the weight ratio of PbO, TeO2, Li2O and Na2O is (30-35): (30-35): (1-3): (1-3).

4. The glass powder for thin Poly layer fine grid silver paste on the back of the battery according to claim 3, characterized in that: The raw materials for preparing the glass powder A include, by weight percentage, 30-35% PbO, 30-35% TeO2, 16-22% Bi2O3, 1.5-5% ZnO, 1-3% Li2O, 2-4% WO3, 1-3% Na2O, and 6-10% SiO2.

5. The glass powder for thin Poly layer fine grid silver paste on the back of the battery according to claim 4, characterized in that: The raw materials for preparing the glass powder B include: PbO, TeO2, WO3 and SiO2, and the weight ratio of PbO, TeO2, WO3 and SiO2 is (25-30): (15-22): (10-15): (8-15).

6. The glass powder for thin Poly layer fine grid silver paste on the back of the battery according to claim 5, characterized in that: The raw materials for preparing the glass powder B include, by weight percentage, 25-30% PbO, 15-22% TeO2, 16-22% Bi2O3, 2-5% ZnO, 2-4% Li2O, 10-15% WO3, 0.5-1% Na2O, 8-15% SiO2 and 1-2% CuO.

7. A method for preparing glass powder for thin Poly layer fine grid silver paste on the back of a battery according to claim 5, characterized in that: The following steps are involved: S1. The raw materials for preparing glass powder A and glass powder B are mixed evenly, respectively put into crucibles, and melted by heat preservation to obtain glass melt A and glass melt B; S2 cold-rolling or water-quenching the glass melt A and the glass melt B respectively to obtain glass slag A and glass slag B; S3: pour glass slag A and glass slag B into ball mill jars respectively, add zirconium balls, and grind them in a planetary ball mill for 0.5-1h; S4 is coarsely ground and further pulverized to obtain glass powder A and glass powder B.

8. The method for preparing glass powder for thin Poly layer fine grid silver paste on the back of battery according to claim 7, characterized in that: In step S1, the insulation temperature is 1000-1200° C., and the insulation time is 20-60 minutes.

9. The method for preparing glass powder for thin Poly layer fine grid silver paste on the back of battery according to claim 7, characterized in that: The further pulverization method in step S4 is selected from one or a combination of mechanical pulverization, air flow pulverization, and impact pulverization.

10. A fine grid silver paste, characterized in that: The preparation raw materials include 2-3 parts by weight of the glass powder according to any one of claims 1 to 6, 86-89 parts by weight of silver powder, 5-10 parts by weight of an organic carrier, and 0.5-1 part by weight of an organic solvent.

Citation Information

Patent Citations

  • Double-component high-contact glass powder for solar front silver paste

    CN111268915A

  • Glass powder for fine grid silver-aluminum paste of TOPCon battery

    CN116444164A

  • Back fine grid silver paste for TOPCon crystalline silicon solar cell as well as preparation method and application of back fine grid silver paste

    CN117038145A

  • Bi-component glass powder for N-type TOPCon and preparation method of bi-component glass powder

    CN117342796A

  • Glass powder for preparing solar cell electrode, paste composition comprising same, solar cell electrode, and solar cell