Heat treatment method of electron beam physical vapor deposition glass microsphere coated coating
Through the heat treatment method of electron beam physical vapor deposition glass microsphere coated coating, the problem of insufficient performance of a single absorbent absorber is solved. The combination strength and performance of the absorber are improved through vacuum heat treatment and multi-stage insulation technology, and the absorption is achieved Improved performance of wave materials.
Patent Information
- Application Number
- CN202411091992.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The absorbent materials of a single absorbent have disadvantages such as narrow frequency bands and unstable absorption performance, which makes it difficult to effectively improve the electromagnetic wave attenuation and dielectric matching characteristics, resulting in a gap between their performance and expected goals.
The heat treatment method of electron beam physical vapor deposition glass microspheres coated with coating is adopted to change the crystal structure and tissue of the glass microspheres through vacuum heat treatment, improving the mechanical properties of the material. The specific steps include heating to 800±50℃ in a vacuum heat treatment furnace, insulated for 2-4 hours, cooling to 600±50℃, and cooling to 250±50℃, and multi-stage insulation at different temperatures, combining cleaning and dehydration and drying. step.
Through multi-stage insulation method, the bonding strength of the cladding layer is improved under low vacuum conditions, the material performance is improved, the performance of the absorbing material is improved, while maintaining the integrity of the microspheres.
Smart Images

Figure CN118930064A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aviation engine coating materials and relates to a heat treatment method for an electron beam physical vapor deposition glass microsphere coating. Background Art
[0002] Absorbent coatings are generally composed of adhesives, absorbents and various additives, among which the absorbent is the main material and directly determines the absorbing performance of the coating. According to the absorbing principle, the important factors affecting the performance of absorbing materials include the impedance matching characteristics of the absorbing materials and the material attenuation characteristics. Among them, improving the attenuation of electromagnetic waves requires improving the electromagnetic loss characteristics of the absorbing materials, while the impedance matching of the absorbing materials requires the absorbing materials to have good dielectric matching characteristics. However, due to the shortcomings of a single absorber such as narrow bandwidth and unstable absorbing performance, the absorbing materials of a single absorber are somewhat far from the expected goal. Therefore, the research on absorber surface modification has received widespread attention. Surface modification is a unique absorber modification method, which is widely used in absorber surface treatment. It can not only improve the bonding strength of absorbing materials, but also reduce the dielectric constant and improve impedance matching and other characteristics, ultimately achieving the purpose of improving the absorbing performance of absorbing materials. Summary of the invention
[0003] The purpose of the present invention is to provide a heat treatment method for an electron beam physical vapor deposition glass microsphere coating, which is designed to improve the mechanical properties of the material by changing the crystal structure and organization of the glass microsphere coating through a vacuum heat treatment method.
[0004] To solve this technical problem, the technical solution of the present invention is:
[0005] Provided is a heat treatment method for an electron beam physical vapor deposition glass microsphere coating, the heat treatment method process is:
[0006] The electron beam physical vapor deposition glass microsphere coating was placed in a vacuum heat treatment furnace and heated to 800±50℃ with a vacuum degree of <1×10 -2 Pa, keep warm for 2-4 hours and then cool to 600±50°C with the furnace, keep warm for 30±5min and then cool to 250±50°C with the furnace, keep warm for 30±5min and then cool to room temperature with the furnace, open the vacuum chamber and take out the coating after cooling to room temperature.
[0007] The coating system is an iron-cobalt-nickel based five-element high entropy absorbing coating FeCoNiXY, wherein X and Y are both metal or transition metal atoms.
[0008] The diameter of the glass microspheres is 100-200 μm. Particle sizes within this range are easier to coat evenly and are easier to prepare, achieving a better balance between cost and effect.
[0009] The electron beam physical vapor deposition process parameters are: evaporation current 0.8-1.2A, rotation speed 5-10RPM, coating layer thickness 10-100μm, glass microsphere diameter 100-200μm.
[0010] The heat treatment method further comprises the steps of cleaning and dehydrating the coating before the heat treatment.
[0011] The cleaning steps are as follows: immersing the electron beam physical vapor deposited glass microspheres coated with iron, cobalt, and nickel-based high entropy absorbing coating in a 10±5% water-based cleaning agent for 30±5 minutes, and then immersing the electron beam physical vapor deposited glass microspheres coated with iron, cobalt, and nickel-based high entropy absorbing coating in deionized water for 30±5 minutes.
[0012] Preferably, the water-based cleaning agent is a degreasing agent with a pH of 7±0.5.
[0013] The dehydration and drying steps are as follows: the electron beam physical vapor deposition glass microspheres coated with the iron-cobalt-nickel-based high entropy absorbing coating are immersed in an organic solvent for 10±5 minutes, then taken out and placed in an oven, and dried at 80±10° C. for 15±5 minutes.
[0014] Preferably, the organic solvent is acetone or ethanol, and the purity is analytical grade.
[0015] The present invention has the following advantages and beneficial effects:
[0016] During the heat treatment process of the present invention, a multi-stage insulation method is adopted. Under low vacuum conditions, by controlling the insulation time and the temperature of each stage, the bonding strength of the coating layer is improved, while the integrity of the microspheres is maintained, ultimately improving the performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions implemented in the present invention, the following is a brief explanation of the drawings required to be used in the examples of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 The appearance changes of the glass microsphere coating before and after the heat treatment of Example 1 are shown in FIG. Figure 1 It can be seen that after being coated with the iron-cobalt-nickel based five-element high entropy absorbing coating, the glass microspheres appear black, indicating that the coating is uniform.
[0019] Figure 2 The figure shows the change in bonding strength of the glass microsphere coatings of Examples 1, 2, 3 and the comparative example.
[0020] from Figure 2 It can be seen that the 800-600-250℃ multi-stage insulation method is adopted to improve the bonding strength of the coating and reach more than 8MPa. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] The features of various aspects of the embodiments of the present invention will be described in detail below. In the following detailed description, many specific details are proposed to provide a comprehensive understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can also be implemented without these specific details.
[0023] The technical solution of the invention will be further described in detail below in conjunction with the embodiments:
[0024] The process conditions in the washing and dehydration and drying steps in the embodiment of the present invention and the comparative example are the same, and the steps are as follows:
[0025] ⑴. Preparation of Fe-Co-Ni based high entropy absorbing coating by electron beam physical vapor deposition glass microsphere coating: wherein, the electron beam physical vapor deposition process parameters are: evaporation current 0.8-1.2A, rotation speed 5-10RPM, coating layer thickness 10-100μm, glass microsphere diameter 100-200μm.
[0026] (2) Cleaning: Soak the electron beam physical vapor deposition glass microspheres coated with iron-cobalt-nickel-based high entropy absorbing coating in 10% water-based cleaning agent for 30 minutes, and then soak the electron beam physical vapor deposition glass microspheres coated with iron-cobalt-nickel-based high entropy absorbing coating in deionized water for 30 minutes; the water-based cleaning agent is a degreasing agent with a pH of 7, and the water-based cleaning agent is specifically an environmentally friendly water-based cleaning agent, a multi-purpose water-based cleaning agent or a strong water-based cleaning agent;
[0027] ⑶, Dehydration and drying: The electron beam physical vapor deposition glass microspheres coated with the iron-cobalt-nickel-based high entropy absorbing coating are immersed in an organic solvent for 10 minutes, then taken out and placed in an oven, and dried at 80°C for 15 minutes. The organic solvent is acetone or ethanol, and the purity is analytical grade;
[0028] Embodiment 1:
[0029] High temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with iron-cobalt-nickel based high entropy absorbing coating (specific composition: FeCoNiTiAl) are placed in a vacuum heat treatment furnace and heated to 850°C with a vacuum degree of 5×10 -3 Pa, then cool to 650°C with the furnace after keeping warm for 2 hours, then cool to 200°C with the furnace after keeping warm for 30 minutes, then cool to room temperature with the furnace after keeping warm for 30 minutes, and then open the vacuum chamber and take out the glass microspheres.
[0030] Embodiment 2:
[0031] High temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with iron-cobalt-nickel based high entropy absorbing coating (specific composition: FeCoNiMnPt) are placed in a vacuum heat treatment furnace and heated to 800°C with a vacuum degree of 3×10 -3 Pa, then cool to 600°C with the furnace after keeping warm for 3 hours, then cool to 250°C with the furnace after keeping warm for 30 minutes, then cool to room temperature with the furnace after keeping warm for 30 minutes, and then open the vacuum chamber and take out the glass microspheres.
[0032] Embodiment 3:
[0033] High temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with iron-cobalt-nickel based high entropy absorbing coating (specific composition: FeCoNiMgZn) are placed in a vacuum heat treatment furnace and heated to 750°C with a vacuum degree of 3×10 -3 Pa, then cool to 550°C with the furnace after keeping warm for 4 hours, then cool to 300°C with the furnace after keeping warm for 30 minutes, then cool to room temperature with the furnace after keeping warm for 30 minutes, and then open the vacuum chamber and take out the glass microspheres.
[0034] Comparative Example:
[0035] High temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with iron-cobalt-nickel based high entropy absorbing coating (specific composition: FeCoNiWAg) are placed in a vacuum heat treatment furnace and heated to 700°C with a vacuum degree of 3×10 -3 Pa, then cool to 500°C with the furnace after keeping warm for 5 hours, then cool to 300°C with the furnace after keeping warm for 30 minutes, then cool to room temperature with the furnace after keeping warm for 30 minutes, and then open the vacuum chamber and take out the glass microspheres.
[0036] like Figure 2The figure shows the change in the bonding strength of the glass microsphere coating of Examples 1, 2, 3 and the comparative example. It can be seen that due to the difference in the insulation temperature parameters and the insulation segmentation parameters, the coating bonding strength in the comparative example is only 5MPa, while the combination of the insulation temperature parameters and the temperature segmentation design parameters in Examples 1, 2 and 3 makes the coating bonding strength above 8MPa. In the heat treatment process of the embodiment of the present invention, a multi-stage insulation method is adopted: heating to 800±50℃ with the furnace--heating for 2-4 hours and then cooling to 600±50℃ with the furnace, heating for 30±5min and then cooling to 250±50℃ with the furnace, heating for 30±5min and then cooling to room temperature with the furnace, under vacuum conditions (vacuum degree <1×10 -2 Pa), by controlling the holding time and the temperature at each stage, the coating layer bonding strength is improved. Figure 2 It can also be seen that, since the maximum insulation parameter of the comparative example is changed compared with other embodiments (the temperature is reduced to 700° C. compared with other embodiments), it is found that the coating bonding strength is greatly reduced.
[0037] In summary, it can be seen that in the heat treatment process of the present invention, a multi-stage heat preservation method is adopted, and the vacuum degree is less than 1×10 -2 Pa conditions, by controlling the insulation time and the temperature of each stage, the bonding strength of the coating layer can be increased to 8MPa, while the integrity of the microspheres can be maintained, ultimately improving the performance of the material.
[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the field can easily think of various equivalent modifications or substitutions within the technical scope disclosed by the present invention, and these modifications or substitutions should all be covered within the protection scope of the present invention.
Claims
1. A heat treatment method for an electron beam physical vapor deposition glass microsphere coating, characterized in that: The heat treatment process is as follows: The electron beam physical vapor deposition glass microsphere coating was placed in a vacuum heat treatment furnace and heated to 800±50℃ with a vacuum degree of <1×10 -2 Pa, keep warm for 2-4 hours and then cool to 600±50°C with the furnace, keep warm for 30±5min and then cool to 250±50°C with the furnace, keep warm for 30±5min and then cool to room temperature with the furnace, open the vacuum chamber and take out the coating after cooling to room temperature.
2. The heat treatment method according to claim 1, characterized in that: The coating system is an iron-cobalt-nickel based five-element high entropy absorbing coating FeCoNiXY, wherein X and Y are both metal or transition metal atoms.
3. The heat treatment method according to claim 1, characterized in that: The diameter of the glass microspheres is 100-200 μm.
4. The heat treatment method according to claim 1, characterized in that: The process parameters of electron beam physical vapor deposition are: evaporation current 0.8-1.2A, rotation speed 5-10RPM, coating thickness 10-100μm, and glass microsphere diameter 100-200μm.
5. The heat treatment method according to claim 1, characterized in that: The method further comprises the steps of cleaning and dehydrating the coating before the heat treatment.
6. The heat treatment method according to claim 5, characterized in that: The cleaning steps are as follows: immersing the electron beam physical vapor deposited glass microspheres coated with iron, cobalt, and nickel-based high entropy absorbing coating in a 10±5% water-based cleaning agent for 30±5 minutes, and then immersing the electron beam physical vapor deposited glass microspheres coated with iron, cobalt, and nickel-based high entropy absorbing coating in deionized water for 30±5 minutes.
7. The heat treatment method according to claim 6, characterized in that: The water-based cleaning agent is a degreasing agent with a pH of 7±0.
5.
8. The heat treatment method according to claim 5, characterized in that: The dehydration and drying steps are as follows: the electron beam physical vapor deposition glass microspheres coated with the iron-cobalt-nickel-based high entropy absorbing coating are immersed in an organic solvent for 10±5 minutes, then taken out and placed in an oven, and dried at 80±10° C. for 15±5 minutes.
9. The heat treatment method according to claim 8, characterized in that: The organic solvent is acetone or ethanol, and its purity is analytical grade.
Citation Information
Patent Citations
Microsphere wave absorption material for building paint electromagnetic radiation prevention and preparation method thereof
CN109437634A
Ceramic microsphere coated nickel coating and preparation method thereof
CN115368166A
Ceramic microsphere coated iron-cobalt-nickel-samarium-neodymium high-entropy coating and preparation method thereof
CN116836576A
Preparation method for surface strengthening of hollow glass beads based on ion exchange
CN117776550A
Nanoparticle-coated multilayer shell microstructures
US9738788B1