Low-calcium silicon-aluminum-based cementing material system and preparation method thereof

Through the low-calcium silicon-based gelling material system, the mixing of spodumene smelting solid waste and cement clinker is used to solve the problem of insufficient carbon emissions and reaction activity in the calcined clay process, and the efficient utilization of lithium resources is achieved and The strength of cement stone is increased.

CN118930079APending Publication Date: 2024-11-12SOUTHWEAT UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410793334.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing low-carbon cementitious material system consumes a large amount of ore resources and fossil fuels during the calcination of clay, resulting in carbon emission problems. The gelling material's reactivity is insufficient, affecting the strength and toughness of cementite.

Method used

Using a low-calcium silicon-aluminum-based gelling material system, the solid waste is smelted by grinding ordinary silicate cement clinker, limestone and spodumene to form a mixed material that does not require high temperature treatment, and improve the reactivity and mechanical properties of the gelling material. .

Benefits of technology

It reduces carbon emissions during the production process, realizes efficient utilization of lithium industrial resources, improves the strength and toughness of cement stone, and ensures a dense interlayer structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930079A_ABST
    Figure CN118930079A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building cementing materials, and discloses a low-calcium silicon-aluminum-based cementing material system and a preparation method of the low-calcium silicon-aluminum-based cementing material system. The low-calcium silicon-aluminum-based cementing material system can be obtained by mixing and grinding the low-calcium silicon-aluminum-based cementing material with a powder grinding material A formed by ordinary Portland cement clinker, limestone and gypsum, and the obtained low-calcium silicon-aluminum-based cementing material does not need to be subjected to high-temperature treatment compared with a cementing material formed by calcined clay, so that carbon emission in the production process can be reduced; efficient utilization of lithium industrial resources is realized; the obtained low-calcium silicon-aluminum-based cementing material has higher reaction activity, can promote the hydration reaction process of the cementing material, improves the silicon chain polymerization degree of C-S-H, ensures that set cement has a compact interlayer structure, and further improves the strength and toughness of the set cement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building cementitious materials, and in particular to a low-calcium silicon-aluminum based cementitious material system and a preparation method thereof. Background Art

[0002] At present, the composite cement system produced by calcining clay and limestone is the most promising low-carbon cementitious material system. The clinker replacement rate of this system exceeds 50%, which not only saves a large amount of silicate cement clinker, indirectly reducing the carbon emissions in the cement production process, but also can be produced in existing cement plants, greatly reducing production and output costs. However, calcining clay requires a large amount of ore resources, and a large amount of fossil fuels are still consumed during the calcination process to provide heat, and there are still some carbon emissions. Summary of the invention

[0003] Based on the above problems, the present invention provides a low-calcium silicon-aluminum-based cementitious material system and a preparation method thereof. The cementitious material does not need to be subjected to high-temperature treatment, can reduce carbon emissions in the production process, and realize efficient utilization of lithium industrial resources; the obtained low-calcium silicon-aluminum-based cementitious material has stronger reaction activity, can promote the hydration reaction process of the cementitious material, improve the silicon chain polymerization degree of CSH, ensure that the cement paste has a dense interlayer structure, and thus improve the strength and toughness of the cement paste.

[0004] In order to achieve the above technical effects, the technical solution adopted by the present invention is:

[0005] A low-calcium silicon-aluminum-based cementitious material system, comprising a mixture of a grinding material A and spodumene smelting solid waste; the grinding material A comprises 40 to 60 parts of ordinary Portland cement clinker, 10 to 20 parts of limestone, and 0 to 5 parts of gypsum, which are ground together to obtain the grinding material A; the spodumene smelting solid waste comprises one or both of spodumene solid waste roasted and leached by sulfuric acid or spodumene solid waste pressurized by nitric acid;

[0006] Wherein, the chemical components of the sulfuric acid roasting and leaching spodumene smelting solid waste include, by mass percentage: 60-65% SiO2, 15-20% Al2O3, 3-5% CaO, 5-8% SO3, 0.05-0.1% Li2O and 0.01%-4% impurity oxides, wherein the impurity oxide B is a combination of one or more oxides of Fe2O3, K2O and MgO;

[0007] The chemical components of the nitric acid pressurized spodumene smelting solid waste include: 75-80% SiO2, 15-20% Al2O3, 0.05-0.1% Li2O, 0.01%-4% impurity oxides, and the impurity oxides C are a combination of one or more oxides of Fe2O3, K2O, CaO, and MgO.

[0008] Furthermore, the gypsum includes one or more of natural gypsum, phosphogypsum, and desulfurized gypsum.

[0009] Furthermore, the limestone has a SiO2 content of less than 2% and a CaO content of more than 53.5%.

[0010] Furthermore, the specific surface area of ​​the low-calcium silicon-aluminum based gelling material is 430 to 470 m 2 / kg.

[0011] In order to achieve the above technical effects, the present invention also provides a method for preparing a low-calcium silicon-aluminum based gelling material system, comprising:

[0012] By weight, 40-60 parts of ordinary Portland cement clinker, 10-20 parts of limestone, and 0-5 parts of gypsum are ground together to obtain a grinding material A;

[0013] The obtained grinding material A is mixed with 20 to 50 parts of spodumene smelting solid waste, and ground to obtain the low-calcium silicon-aluminum based gelling material, wherein the spodumene smelting solid waste includes one or both of spodumene solid waste leached by sulfuric acid roasting or spodumene solid waste pressurized by nitric acid;

[0014] Wherein, the chemical components of the sulfuric acid roasting and leaching spodumene smelting solid waste include, by mass percentage: 60-65% SiO2, 15-20% Al2O3, 3-5% CaO, 5-8% SO3, 0.05-0.1% Li2O and 0.01%-4% impurity oxides, wherein the impurity oxide B is a combination of one or more oxides of Fe2O3, K2O and MgO;

[0015] The chemical components of the nitric acid pressurized spodumene smelting solid waste include: 75-80% SiO2, 15-20% Al2O3, 0.05-0.1% Li2O, 0.01%-4% impurity oxides, and the impurity oxides C are a combination of one or more oxides of Fe2O3, K2O, CaO, and MgO.

[0016] Furthermore, the gypsum includes one or more of natural gypsum, phosphogypsum, and desulfurized gypsum.

[0017] Furthermore, the limestone has a SiO2 content of less than 2% and a CaO content of more than 53.5%.

[0018] Furthermore, in the process of grinding common Portland cement clinker, limestone and gypsum together, it is ensured that the materials discharged from the mill are fully mixed and uniformly mixed while the fineness meets the requirements of common Portland cement.

[0019] Compared with the prior art, the present invention has the following beneficial effects: compared with the cementitious material formed by calcined clay, the low-calcium silicon-aluminum-based cementitious material system of the present invention does not need to be subjected to high-temperature treatment, can reduce carbon emissions in the production process, and realize efficient utilization of lithium industrial resources; the obtained low-calcium silicon-aluminum-based cementitious material system has stronger reaction activity, can promote the hydration reaction process of the cementitious material, improve the silicon chain polymerization degree of CSH, ensure that the cement paste has a dense interlayer structure, and thus improve the strength and toughness of the cement paste. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XRD diagram of the low-calcium silicon-aluminum based gelling material sample hydrated for 28 days in Example 2.

[0021] Figure 2 This is the SEM image of the low-calcium silicon-aluminum based cementitious material sample hydrated for 28 days in Example 2. DETAILED DESCRIPTION

[0022] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0023] Example 1

[0024] A low-calcium silicon-aluminum-based cementitious material system, comprising a mixture of a grinding material A and spodumene smelting solid waste; the grinding material A comprises 40 to 60 parts of ordinary Portland cement clinker, 10 to 20 parts of limestone, and 0 to 5 parts of gypsum, which are ground together to obtain the grinding material A; the spodumene smelting solid waste comprises one or both of spodumene solid waste roasted and leached by sulfuric acid or spodumene solid waste pressurized by nitric acid;

[0025] Wherein, the chemical components of the sulfuric acid roasting and leaching spodumene smelting solid waste include, by mass percentage: 60-65% SiO2, 15-20% Al2O3, 3-5% CaO, 5-8% SO3, 0.05-0.1% Li2O and 0.01%-4% impurity oxides, wherein the impurity oxide B is a combination of one or more oxides of Fe2O3, K2O and MgO;

[0026] The chemical components of the nitric acid pressurized spodumene smelting solid waste include: 75-80% SiO2, 15-20% Al2O3, 0.05-0.1% Li2O, 0.01%-4% impurity oxides, and the impurity oxides C are a combination of one or more oxides of Fe2O3, K2O, CaO, and MgO.

[0027] In this embodiment, spodumene smelting solid waste is used as the raw material of the low-calcium silicon-aluminum-based cementitious material system, and is mixed and ground with a powder abrasive A formed by ordinary Portland cement clinker, limestone, and gypsum to obtain a low-calcium silicon-aluminum-based cementitious material system, which does not need to be treated at high temperature, reduces carbon emissions in the production process, and solves the problem of efficient utilization of lithium industrial resources. In addition, spodumene smelting solid waste includes sulfuric acid roasting and leaching spodumene solid waste and nitric acid pressurized spodumene solid waste, and its main mineral components include β-spodumene, quartz, and feldspar. Among them, the hydrogen ions / lithium ions in β-spodumene have strong cation exchangeability and large cation exchange capacity, which can improve the hydration reaction between spodumene smelting solid waste and Ca 2+ 、Al 3+ and Fe 3+ The interaction ability of the β-spodumene improves the hydration ability of the low-calcium silicon-aluminum based cementitious material; and the lithium ions / hydrogen ions in the β-spodumene structure have two equivalent positions in the structure, but only one position appears in the actual crystal, which makes the lithium ions / hydrogen ions and oxygen atoms four times coordinated to produce deformed lithium oxygen tetrahedrons or hydrogen oxygen tetrahedrons, resulting in lattice distortion of β-spodumene, so that the Al-O bonds and Si-O bonds in the β-spodumene structure are in a metastable state, and the metastable Al-O bonds and Si-O bonds are accelerated to break under hydration. The cracking of CSH promotes the hydration reaction of cementitious materials, increases the polymerization degree of silicon chains of CSH, and enhances the mechanical properties of cementitious materials. In addition, the active alumina contained in spodumene smelting solid waste can work together with gypsum and calcium carbonate to stabilize the calcium aluminate in the hydration products and promote the formation of CO3-AFm phase products, which is beneficial to the development of mechanical properties of cementitious system. Moreover, the doping of AFm phase on the surface and interlayer of CSH can improve the deformation ability of CSH, densify the interlayer structure, and promote the development of strength and toughness of cement paste.

[0028] Therefore, compared with the cementitious material formed by calcined clay, the low-calcium silicon-aluminum-based cementitious material in this embodiment does not need to be subjected to high-temperature treatment, can reduce carbon emissions in the production process, and realize efficient utilization of lithium industrial resources; the obtained low-calcium silicon-aluminum-based cementitious material has stronger reactivity, can promote the hydration reaction process of the cementitious material, increase the silicon chain polymerization degree of CSH, ensure that the cement paste has a dense interlayer structure, and thereby improve the strength and toughness of the cement paste.

[0029] The gypsum in this embodiment includes one or more of natural gypsum, phosphogypsum, and desulfurized gypsum; the SiO2 content of the limestone is less than 2%, and the CaO content is greater than 53.5%. The specific surface area of ​​the low-calcium silicon-aluminum based cementitious material is 430-470 m 2 / kg.

[0030] Based on the same inventive concept, this embodiment also provides a method for preparing a low-calcium silicon-aluminum based gelling material system, comprising:

[0031] By weight, 40-60 parts of ordinary Portland cement clinker, 10-20 parts of limestone, and 0-5 parts of gypsum are ground together to obtain a grinding material A;

[0032] The obtained grinding material A is mixed with 20 to 50 parts of spodumene smelting solid waste, and ground to obtain the low-calcium silicon-aluminum-based gelling material. The spodumene smelting solid waste includes one or both of spodumene solid waste roasted and leached by sulfuric acid or spodumene solid waste pressurized by nitric acid.

[0033] Example 2

[0034] A low-calcium silicon-aluminum based gelling material system, the preparation method of which is as follows:

[0035] Step 1: Grind ordinary Portland cement clinker, limestone, phosphogypsum and desulfurized gypsum in a weight percentage of 75:20:2.5:2.5 to a specific surface area of ​​350m 2 / kg, and obtain powder abrasive A.

[0036] Step 2: Grind the nitric acid pressure-leached spodumene solid waste to a specific surface area of ​​460 m 2 / kg.

[0037] Step 3: Grind the obtained powder A and nitric acid pressure leached spodumene solid waste to 450 m 2 / kg, a low-calcium silicon-aluminum based gelling material system was obtained.

[0038] Step 4. Prepare cement mortar with the low-calcium silicon-aluminum-based cementitious material obtained in step 3 according to GB / T-17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and place it in a triple test mold of 40*40*160mm. Curing the prepared sample in a standard curing box at 20±1℃ and relative humidity>90% for 28 days.

[0039] Example 3

[0040] Step 1: Grind ordinary Portland cement clinker, limestone and natural gypsum in a weight percentage ratio of 75:20:5 to a specific surface area of ​​340m 2 / kg, and obtain powder abrasive A.

[0041] Step 2: Grind the nitric acid pressure-leached spodumene solid waste to a specific surface area of ​​450 m 2 / kg.

[0042] Step 3: Grind the obtained powder A and nitric acid pressure leached spodumene solid waste to 460 m 2 / kg, a low-calcium silicon-aluminum based gelling material system was obtained.

[0043] Step 4. Prepare cement mortar with the low-calcium silicon-aluminum-based cementitious material obtained in step 3 according to GB / T-17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and place it in a triple test mold of 40*40*160mm. Curing the prepared sample in a standard curing box at 20±1℃ and relative humidity>90% for 28 days.

[0044] Example 4

[0045] Step 1: Grind ordinary Portland cement clinker, limestone and phosphogypsum in a weight percentage ratio of 75:20:5 to a specific surface area of ​​330m 2 / kg, and obtain powder abrasive A.

[0046] Step 2: Grind the sulfuric acid roasted spodumene solid waste to a specific surface area of ​​470 m 2 / kg.

[0047] Step 3: Grind the obtained powder A and sulfuric acid roasted spodumene solid waste to 440 m 2 / kg, a low-calcium silicon-aluminum based gelling material system was obtained.

[0048] Step 4. Prepare cement mortar with the low-calcium silicon-aluminum-based cementitious material obtained in step 3 according to GB / T-17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and place it in a triple test mold of 40*40*160mm. Curing the prepared sample in a standard curing box at 20±1℃ and relative humidity>90% for 28 days.

[0049] Example 5

[0050] Step 1: Grind ordinary Portland cement clinker, limestone and desulfurized gypsum in a weight percentage of 75:20:5 to a specific surface area of ​​350m 2 / kg, and obtain powder abrasive A.

[0051] Step 2: Grind the nitric acid pressure-leached spodumene solid waste to a specific surface area of ​​480 m 2 / kg.

[0052] Step 3: Grind the obtained powder A and sulfuric acid roasted spodumene solid waste to 460 m 2 / kg, a low-calcium silicon-aluminum based gelling material system was obtained.

[0053] Step 4. Prepare cement mortar with the low-calcium silicon-aluminum-based cementitious material obtained in step 3 according to GB / T-17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and place it in a triple test mold of 40*40*160mm. Curing the prepared sample in a standard curing box at 20±1℃ and relative humidity>90% for 28 days.

[0054] Example 6

[0055] Step 1: Grind ordinary Portland cement clinker, limestone, natural gypsum and desulfurized gypsum in a weight percentage of 75:20:2.5:2.5 to a specific surface area of ​​340m 2 / kg, and obtain powder abrasive A.

[0056] Step 2: Grind the nitric acid pressure-leached spodumene solid waste to a specific surface area of ​​490 m 2 / kg.

[0057] Step 3: Grind the obtained powder A and nitric acid pressure leached spodumene solid waste to 450 m 2 / kg, a low-calcium silicon-aluminum based gelling material system was obtained.

[0058] Step 4. Prepare cement mortar with the low-calcium silicon-aluminum-based cementitious material obtained in step 3 according to GB / T-17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and place it in a triple test mold of 40*40*160mm. Curing the prepared sample in a standard curing box at 20±1℃ and relative humidity>90% for 28 days.

[0059] Comparison Example

[0060] Step 1: Grind 50 parts of ordinary Portland cement clinker and 50 parts of limestone together to a specific surface area of ​​450m 2 / kg, a low-calcium silicon-aluminum based gelling material was obtained.

[0061] Step 2. Prepare cement mortar with the low-calcium silicon-aluminum-based cementitious material obtained in step 1 according to GB / T-17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and place it in a triple test mold of 40*40*160mm. Curing the prepared sample in a standard curing box at 20±1℃ and relative humidity>90% for 28 days.

[0062] The mechanical properties of the samples prepared in Examples 2-6 and the comparative example after curing for 28 days in a standard curing box at 20±1°C and relative humidity>90% are shown in Table 1:

[0063] Table 1 Mechanical properties of cementitious materials

[0064] Example Test block size Compressive strength(MPa) Flexural strength(MPa) Example 2 40*40*160mm 35.4 5.9 Example 3 40*40*160mm 38.8 6.7 Example 4 40*40*160mm 36.5 6.3 Example 5 40*40*160mm 35.2 6.2 Example 6 40*40*160mm 39.6 6.9 Comparison example 40*40*160mm 18.7 3.6

[0065] The low-calcium silicon-aluminum based cementitious material sample hydrated for 28 days prepared in Example 2 was characterized by XRD and SEM. Figure 1 This is the XRD diffraction pattern of the sample of the low-calcium silicon-aluminum based gelling material system of Example 2 that was hydrated for 28 days. Figure 2This is a SEM image of a 28-day hydrated sample of the low-calcium silicon-aluminum-based cementitious material system in Example 2. The test results show that the hydration products in the early stage of the reaction are mainly CSH and CH (calcium hydroxide). As the hydration reaction proceeds, the active aluminosilicate in the lithium extraction waste residue undergoes a secondary hydration reaction with CH to generate more structurally stable ettringite phases and monocarbonate phases, which synergize hydration and promote strength improvement.

[0066] This embodiment uses spodumene smelting solid waste as the preparation raw material, so that the content of cement clinker in the system is less than 55%, which greatly reduces the carbon emissions in the cement production process. From the perspective of solving scientific problems, this method solves the problem of slow development of mechanical properties of low-carbon cementitious materials. From the perspective of preparation technology, it solves the problem of roasting and activating raw materials in low-carbon cementitious materials, simplifies the preparation process, and further reduces carbon emissions. From the perspective of economy, the cost price of the solid waste raw materials used is lower than that of natural mineral materials.

[0067] The above is an embodiment of the present invention. The above embodiments and the specific parameters in the embodiments are only for the purpose of clearly describing the invention verification process, and are not intended to limit the patent protection scope of the present invention. The patent protection scope of the present invention is still subject to its claims. Any equivalent structural changes made by using the contents of the description and drawings of the present invention should be included in the protection scope of the present invention.

Claims

1. A low-calcium silicon-aluminum based gelling material system, characterized in that: A mixed material comprising a grinding material A and spodumene smelting solid waste; the grinding material A comprises 40 to 60 parts of ordinary Portland cement clinker, 10 to 20 parts of limestone, and 0 to 5 parts of gypsum, which are ground together to obtain the grinding material A; the spodumene smelting solid waste comprises one or both of spodumene solid waste leached by sulfuric acid roasting or spodumene solid waste pressurized by nitric acid; Wherein, the chemical components of the sulfuric acid roasting and leaching spodumene smelting solid waste include, by mass percentage: 60-65% SiO2, 15-20% Al2O3, 3-5% CaO, 5-8% SO3, 0.05-0.1% Li2O and 0.01%-4% impurity oxides, wherein the impurity oxide B is a combination of one or more oxides of Fe2O3, K2O and MgO; The chemical components of the nitric acid pressurized spodumene smelting solid waste include: 75-80% SiO2, 15-20% Al2O3, 0.05-0.1% Li2O, 0.01%-4% impurity oxides, and the impurity oxides C are a combination of one or more oxides of Fe2O3, K2O, CaO, and MgO.

2. The low-calcium silicon-aluminum based gelling material system according to claim 1, characterized in that: The gypsum includes one or more of natural gypsum, phosphogypsum and desulfurized gypsum.

3. The low-calcium silicon-aluminum based gelling material system according to claim 1, characterized in that: The limestone has a SiO2 content of less than 2% and a CaO content of more than 53.5%.

4. The low-calcium silicon-aluminum based gelling material system according to claim 1, characterized in that: The specific surface area of ​​the low-calcium silicon-aluminum based gelling material is 430 to 470 m 2 / kg.

5. A method for preparing a low-calcium silicon-aluminum based gelling material system, characterized in that: include: By weight, 40-60 parts of ordinary Portland cement clinker, 10-20 parts of limestone, and 0-5 parts of gypsum are ground together to obtain a grinding material A; The obtained grinding material A is mixed with 20 to 50 parts of spodumene smelting solid waste, and ground to obtain the low-calcium silicon-aluminum based gelling material, wherein the spodumene smelting solid waste includes one or both of spodumene solid waste leached by sulfuric acid roasting or spodumene solid waste pressurized by nitric acid; Wherein, the chemical components of the sulfuric acid roasting and leaching spodumene smelting solid waste include, by mass percentage: 60-65% SiO2, 15-20% Al2O3, 3-5% CaO, 5-8% SO3, 0.05-0.1% Li2O and 0.01%-4% impurity oxides, wherein the impurity oxide B is a combination of one or more oxides of Fe2O3, K2O and MgO; The chemical components of the nitric acid pressurized spodumene smelting solid waste include: 75-80% SiO2, 15-20% Al2O3, 0.05-0.1% Li2O, 0.01%-4% impurity oxides, and the impurity oxides C are a combination of one or more oxides of Fe2O3, K2O, CaO, and MgO.

6. The method for preparing a low-calcium silicon-aluminum based gelling material system according to claim 5, characterized in that: The gypsum includes one or more of natural gypsum, phosphogypsum and desulfurized gypsum.

7. The method for preparing a low-calcium silicon-aluminum based gelling material system according to claim 5, characterized in that: The limestone has a SiO2 content of less than 2% and a CaO content of more than 53.5%.

8. The method for preparing a low-calcium silicon-aluminum based gelling material system according to claim 5, characterized in that: In the process of grinding ordinary Portland cement clinker, limestone and gypsum together, it is ensured that the materials discharged from the mill are fully mixed and uniformly while the fineness meets the requirements of ordinary Portland cement.

Citation Information

Patent Citations

  • Eco-friendly cement and preparation method thereof

    CN107188436A

  • High-strength white cement and preparation process thereof

    CN110683773A

  • Method for producing early strength cement from lithium slag

    CN114249549A

  • Lithium-doped oil well cement and preparation method thereof

    CN118084364A