Cement-like cementing material based on coal-based solid waste and preparation method of cement-like cementing material

By preparing cement-like cementitious materials based on coal-based solid waste, using solid waste such as steel slag and slag, the problems of high cement use cost and environmental pollution are solved, low-cost and environmentally friendly preparation of cement materials are achieved, and solids are improved Waste utilization rate.

CN118930080AInactive Publication Date: 2024-11-12HENAN POLYTECHNIC UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411097436.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The use of cement in the prior art leads to high cost of building materials and environmental pollution, and fails to effectively utilize a large amount of solid waste such as steel slag and slag.

Method used

The cement-like cementitious material based on coal-based solid waste is used, and its composition includes steel slag powder, slag powder, cement clinker and desulfurization gypsum powder. It is prepared by drying, grinding and mixing evenly mixing to form a low-cost and environmentally friendly Gelatinized material.

Benefits of technology

It overcomes the problems of high cement use cost and environmental pollution, effectively utilizes solid waste, reduces the harm of solid waste accumulation, improves resource utilization, and provides economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a cement-like cementing material based on coal-based solid waste and a preparation method of the cement-like cementing material, and belongs to the technical field of cementing material preparation. Comprising the following components in percentage by mass: 6-12% of steel slag powder, 55-75% of slag powder, 5-20% of cement clinker and 3-12% of desulfurized gypsum powder. The steel slag powder comprises, by mass, 35%-40% of calcium oxide, 14%-20% of silicon dioxide, 20%-25% of ferric oxide, 1%-7% of aluminum oxide and 8%-14% of magnesium oxide. The slag powder comprises the following components in percentage by mass: 35%-40% of calcium oxide, 30%-34% of silicon dioxide, 1%-5% of ferric oxide, 13%-17% of aluminum oxide and 7%-13% of magnesium oxide. The cement clinker comprises the following components in percentage by mass: 60%-70% of calcium oxide, 20%-24% of silicon dioxide, 4%-8% of aluminum oxide, 2%-5% of ferric oxide and 1%-4% of magnesium oxide. The mass content of calcium sulfate dihydrate in the desulfurized gypsum is 93%-99%. The prepared cementing material is simple in component composition, rich in raw materials and low in price, the defects of high cost and indirect environmental pollution caused by direct use of cement are overcome, and higher economic benefits can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cementitious material preparation, and in particular to a cement-like cementitious material based on coal-based solid waste and a preparation method thereof. Background Art

[0003] Cement, as the most commonly used cementitious material, is the basic raw material of building materials and has been at a high plateau for a long time. The use of cement not only increases the cost of building materials, but also indirectly causes environmental pollution. The preparation of cement-like cementitious materials using bulk solid waste such as steel slag, slag, and desulfurized gypsum has become the focus of research and development in this field. Summary of the invention

[0004] The technical problem to be solved by the present invention is to address the deficiencies of the above-mentioned prior art. The purpose of the present invention is to propose a cement-like cementitious material based on coal-based solid waste and a preparation method thereof. The cement-like cementitious material based on coal-based solid waste has a simple component structure, abundant raw materials used, and low price. It overcomes the defects of high cost and indirect environmental pollution caused by direct use of cement, and effectively utilizes a large amount of solid waste such as steel slag, slag, desulfurization gypsum, etc., turning waste into treasure.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 6%-12% of steel slag powder, 55%-75% of slag powder, 5%-20% of cement clinker and 3%-12% of desulfurized gypsum powder.

[0007] Preferably, the steel slag powder comprises, by mass percentage, 35%-40% calcium oxide, 14%-20% silicon dioxide, 20%-25% iron oxide, 1%-7% aluminum oxide and 8%-14% magnesium oxide.

[0008] Preferably, the slag powder comprises, by mass percentage, 35%-40% calcium oxide, 30%-34% silicon dioxide, 1%-5% iron oxide, 13%-17% aluminum oxide and 7%-13% magnesium oxide.

[0009] Preferably, the cement clinker comprises, by mass percentage, 60%-70% calcium oxide, 20%-24% silicon dioxide, 4%-8% aluminum oxide, 2%-5% iron oxide, and 1%-4% magnesium oxide.

[0010] Further preferably, the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 93%-99%.

[0011] As a further preferred technical solution of the present invention, the cement-like cementitious material based on coal-based solid waste comprises the following components in mass percentage: 8%-10% steel slag powder, 65%-75% slag powder, 15%-20% cement clinker and 5%-10% desulfurized gypsum powder. The raw material composition in this mass percentage can further improve the cohesiveness and early strength of the cementitious material.

[0012] Another technical solution of the present invention is:

[0013] A method for preparing a cement-like cementitious material based on coal-based solid waste, the preparation method comprising:

[0014] Step 1. Drying, powdering and sieving the steel slag and ore slag in an oven respectively;

[0015] Step 2. crushing the cement clinker and then sieving it;

[0016] Step 3. crushing the desulfurized gypsum and sieving it;

[0017] Step 4: weigh the steel slag powder, slag powder, cement clinker and desulfurized gypsum powder according to the mixing ratio, mix them evenly and stir to obtain a cementitious material.

[0018] Preferably, in step 1, the steel slag and ore slag are dried in an oven at 105-115° C. for 3-6 hours, ground in a φ500mm*500mm mill, and then sieved to 200 mesh for later use.

[0019] Preferably, in step 2, the cement clinker is sieved through a 3 mm sieve for later use.

[0020] Further preferably, in the step 3, the desulfurized gypsum is sieved through a 3 mm sieve for later use.

[0021] Compared with the prior art, the present invention has the following technical effects:

[0022] 1: The cementitious material prepared by the present invention has a simple component composition, a simple preparation process, and uses abundant raw materials at a low price, thus overcoming the defects of high cost and indirect environmental pollution caused by direct use of cement, and can replace silicate cement to obtain huge economic benefits.

[0023] 2: The present invention effectively utilizes a large amount of solid waste such as steel slag, slag, desulfurized gypsum, etc., reduces the environmental harm caused by the accumulation of solid waste, improves the comprehensive utilization value of solid waste, solves the problem of resource utilization of solid waste, and has important social and environmental benefits. DETAILED DESCRIPTION

[0024] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments; in the following description, specific details such as specific configurations are provided only to help fully understand the embodiments of the present invention. Therefore, it should be clear to those skilled in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present invention.

[0025] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0026] Embodiment 1:

[0027] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 10% of steel slag powder, 75% of slag powder, 5% of cement clinker and 10% of desulfurized gypsum powder.

[0028] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 35% calcium oxide, 20% silicon dioxide, 25% iron oxide, 6% aluminum oxide and 14% magnesium oxide by mass percentage; the slag powder includes 35% calcium oxide, 34% silicon dioxide, 2% iron oxide, 16% aluminum oxide and 13% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 60% calcium oxide, 24% silicon dioxide, 8% aluminum oxide, 5% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 93%. The above-mentioned steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above-mentioned mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0029] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0030] Embodiment 2:

[0031] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 10% of steel slag powder, 65% of slag powder, 20% of cement clinker and 5% of desulfurized gypsum powder.

[0032] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 40% calcium oxide, 18% silicon dioxide, 23% iron oxide, 7% aluminum oxide and 12% magnesium oxide by mass percentage; the slag powder includes 40% calcium oxide, 32% silicon dioxide, 4% iron oxide, 14% aluminum oxide and 10% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 70% calcium oxide, 22% silicon dioxide, 4% aluminum oxide, 2% iron oxide and 2% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The above-mentioned steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above-mentioned mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0033] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0034] Embodiment 3:

[0035] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 11% of steel slag powder, 74% of slag powder, 10% of cement clinker and 5% of desulfurized gypsum powder.

[0036] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 37% calcium oxide, 19% silicon dioxide, 23% iron oxide, 7% aluminum oxide and 14% magnesium oxide by mass percentage; the slag powder includes 37% calcium oxide, 32% silicon dioxide, 3% iron oxide, 16% aluminum oxide and 11% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 65% calcium oxide, 22% silicon dioxide, 6% aluminum oxide, 4% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The above steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0037] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0038] Embodiment 4:

[0039] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 12% of steel slag powder, 68% of slag powder, 14% of cement clinker and 6% of desulfurized gypsum powder.

[0040] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 38% calcium oxide, 19% silicon dioxide, 24% iron oxide, 6% aluminum oxide and 13% magnesium oxide by mass percentage; the slag powder includes 37% calcium oxide, 34% silicon dioxide, 2% iron oxide, 16% aluminum oxide and 11% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 64% calcium oxide, 22% silicon dioxide, 6% aluminum oxide, 5% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0041] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0042] Embodiment 5:

[0043] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 9% of steel slag powder, 70% of slag powder, 17% of cement clinker and 4% of desulfurized gypsum powder.

[0044] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 38% calcium oxide, 19% silicon dioxide, 24% iron oxide, 6% aluminum oxide and 13% magnesium oxide by mass percentage; the slag powder includes 37% calcium oxide, 34% silicon dioxide, 2% iron oxide, 16% aluminum oxide and 11% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 64% calcium oxide, 22% silicon dioxide, 6% aluminum oxide, 5% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0045] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0046] Embodiment 6:

[0047] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 8% of steel slag powder, 67% of slag powder, 20% of cement clinker and 5% of desulfurized gypsum powder.

[0048] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 38% calcium oxide, 19% silicon dioxide, 24% iron oxide, 6% aluminum oxide and 13% magnesium oxide by mass percentage; the slag powder includes 37% calcium oxide, 34% silicon dioxide, 2% iron oxide, 16% aluminum oxide and 11% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 64% calcium oxide, 22% silicon dioxide, 6% aluminum oxide, 5% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0049] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0050] Embodiment 7:

[0051] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 6% of steel slag powder, 74% of slag powder, 15% of cement clinker and 5% of desulfurized gypsum powder.

[0052] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 38% calcium oxide, 19% silicon dioxide, 24% iron oxide, 6% aluminum oxide and 13% magnesium oxide by mass percentage; the slag powder includes 37% calcium oxide, 34% silicon dioxide, 2% iron oxide, 16% aluminum oxide and 11% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 64% calcium oxide, 22% silicon dioxide, 6% aluminum oxide, 5% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0053] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0054] Embodiment 8:

[0055] A cement-like cementitious material based on coal-based solid waste comprises the following components in percentage by mass: 10% of steel slag powder, 70% of slag powder, 15% of cement clinker and 5% of desulfurized gypsum powder.

[0056] The steel slag and slag are dried in an oven at 110°C for 5 hours, ground in a φ500mm*500mm mill and then sieved through 200 meshes; the steel slag powder includes 38% calcium oxide, 19% silicon dioxide, 24% iron oxide, 6% aluminum oxide and 13% magnesium oxide by mass percentage; the slag powder includes 37% calcium oxide, 34% silicon dioxide, 2% iron oxide, 16% aluminum oxide and 11% magnesium oxide by mass percentage. The cement clinker and desulfurized gypsum are sieved through a 3mm sieve respectively; the cement clinker includes 64% calcium oxide, 22% silicon dioxide, 6% aluminum oxide, 5% iron oxide and 3% magnesium oxide by mass percentage; the mass content of calcium sulfate dihydrate in the desulfurized gypsum is 99%. The steel slag powder, slag powder, cement clinker and desulfurized gypsum powder are mixed and stirred evenly according to the above mass percentages to obtain a cement-like cementitious material based on coal-based solid waste.

[0057] The cementitious material and pure water were mixed evenly in a ratio of 2:1, injected into a 100mm×100mm×100mm cubic mold, and then placed on a vibration table for 5 minutes. The sample was demoulded after 4 hours and placed in a curing box at a temperature of 20°C and a relative humidity of 95% for 3 to 28 days of curing. The unconfined compressive strength of the cementitious material test blocks was tested after 3 days and 28 days of curing.

[0058] The water-cement ratio, demoulding time, and unconfined compressive strength of the cementitious material test blocks obtained in Examples 1-8 after curing for 3 days and 28 days are shown in Table 1.

[0059] Table 1

[0060]

[0061] As can be seen from Table 1, the preparation conditions and steps of each group of Examples 1-8 are the same, the water-cement ratio and the demoulding time are also exactly the same, and the cement-like cementitious materials based on coal-based solid waste disclosed by the present invention all have good compressive strength tests. The cement-like cementitious materials based on coal-based solid waste obtained by the present invention can be used as a substitute for cement, overcoming the problems of high cost and indirect environmental pollution caused by the use of cement, while effectively utilizing a large amount of solid waste such as steel slag and slag, thereby improving the comprehensive utilization value of solid waste.

[0062] This embodiment provides that those skilled in the art to which this application belongs can make various modifications or supplements to the described specific embodiments or replace them in a similar manner, but they will not deviate from the inventive concept of this application or exceed the scope defined by the attached claims.

Claims

1. A cement-like cementitious material based on coal-based solid waste, characterized in that: The invention comprises the following components in percentage by mass: 6%-12% of steel slag powder, 55%-75% of slag powder, 5%-20% of cement clinker and 3%-12% of desulfurized gypsum powder.

2. The cement-like cementitious material based on coal-based solid waste according to claim 1, characterized in that: The steel slag powder comprises 35%-40% of calcium oxide, 14%-20% of silicon dioxide, 20%-25% of iron oxide, 1%-7% of aluminum oxide and 8%-14% of magnesium oxide in terms of mass percentage.

3. The cement-like cementitious material based on coal-based solid waste according to claim 2, characterized in that: The slag powder comprises 35%-40% of calcium oxide, 30%-34% of silicon dioxide, 1%-5% of iron oxide, 13%-17% of aluminum oxide and 7%-13% of magnesium oxide in terms of mass percentage.

4. The cement-like cementitious material based on coal-based solid waste according to claim 3, characterized in that: The cement clinker comprises 60%-70% of calcium oxide, 20%-24% of silicon dioxide, 4%-8% of aluminum oxide, 2%-5% of iron oxide and 1%-4% of magnesium oxide in terms of mass percentage.

5. The cement-like cementitious material based on coal-based solid waste according to claim 4, characterized in that: The mass content of calcium sulfate dihydrate in the desulfurized gypsum is 93%-99%.

6. The cement-like cementitious material based on coal-based solid waste according to claim 5, characterized in that: The mass percentages of the components in the cement-like cementitious material are: 8%-10% of steel slag powder, 65%-75% of slag powder, 15%-20% of cement clinker and 5%-10% of desulfurized gypsum powder.

7. A method for preparing a cement-like cementitious material based on coal-based solid waste, characterized in that: The steps include: Step 1. Drying, powdering and sieving the steel slag and ore slag in an oven respectively; Step 2. crushing the cement clinker and then sieving it; Step 3. crushing the desulfurized gypsum and sieving it; Step 4: weigh the steel slag powder, slag powder, cement clinker and desulfurized gypsum powder according to the mixing ratio, mix them evenly and stir to obtain a cementitious material.

8. The method for preparing a cement-like cementitious material based on coal-based solid waste according to claim 7, characterized in that: In the step 1, the steel slag and the ore slag are dried in an oven at 105-115° C. for 3-6 hours, ground in a φ500mm*500mm mill, and then sieved to 200 mesh for later use.

9. The method for preparing a cement-like cementitious material based on coal-based solid waste according to claim 8, characterized in that: In the step 2, the cement clinker is sieved through a 3 mm sieve for later use.

10. A method for preparing a cement-like cementitious material based on coal-based solid waste according to claim 8 or 9, characterized in that: In the step 3, the desulfurized gypsum is sieved through a 3 mm sieve for later use.

Citation Information

Patent Citations

  • Desulfurization gypsum clinker-free steel slag cement

    CN102079635A

  • Method for producing road water permeable brick by using steel slag

    CN102850025A

  • Cementing material for modifying bulk filling body as well as preparation method and application of cementing material

    CN113149478A

  • AU2020101522A4