Method for preparing green cementing material through multi-waste synergistic recycling and green cementing material

By grinding and calcining calcium-based waste residue, silicon-aluminum-based waste residue and mixing it with desulfurization gypsum powder, a high-solid waste residue do not need to be added to raw ore cement clinker is prepared, which solves the environment of traditional sludge curing methods. The problems of high pollution and energy consumption have achieved effective curing of sludge and soft soil and elimination of pollutants.

CN118930085APending Publication Date: 2024-11-12PINGAN ELECTRICAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988655.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the sludge curing method covers a large area and has high energy consumption. In addition, the amount of bulk solid waste added in traditional cementitious materials is low, and raw ore cement clinker and other additives are required, which fails to effectively solve environmental pollution and greenness. Environmental protection issues.

Method used

By grinding calcium-based waste residue and silicon-aluminum-based waste residue, calcining and grinding, mixing with desulfurized gypsum powder, adding modifiers for stirring, a green gelling material without adding raw ore cement clinker was prepared, and the solid waste residue was mixed to 92.5% The above is to use physical excitation methods to significantly reduce environmental pollution.

Benefits of technology

It significantly improves the resource utilization rate of solid waste and reduces the pressure of environmental pollution. The prepared green gelling materials have good curing and heavy metal and odor elimination effects on silt and soft soil, and meet the requirements of low-carbon sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930085A_ABST
    Figure CN118930085A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a green cementing material through multi-waste synergetic recycling and the green cementing material. The green cementing material is prepared from the following raw materials in parts by mass: 1-10 parts of sodium silicate, 1-10 parts of sodium silicate and 1-10 parts of sodium silicate. Comprising the following components in parts by weight: 30.0 to 50.0 parts of calcium-based active mineral powder, 10.0 to 20.0 parts of desulfurized gypsum, 10.0 to 20.0 parts of silicon-aluminum-based waste residue, 20.0 to 40.0 parts of active hydraulic gel, 1.0 to 2.0 parts of a first modifier and 3.0 to 6.0 parts of a second modifier. The preparation method comprises the following preparation steps: mixing the calcium-based waste residue and the silicon-aluminum-based waste residue, calcining, grinding to obtain an active hydraulic gel, mixing the active hydraulic gel with the active mineral powder and the desulfurized gypsum powder, adding the naphthalene sulfonate and the clay mineral powder, and carrying out rotary stirring to obtain the green cementing material without an exciting agent. The green cementing material prepared by the preparation method disclosed by the invention has a good curing effect on to-be-cured soft soil such as sludge, has good curing and eliminating effects on heavy metals and stink in the soft soil such as the sludge, and has obvious advantages compared with similar products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of environmental protection technology, and belongs to the field of resource utilization of bulk solid waste and sludge solidification, and specifically to a method for preparing green cementitious materials through the coordinated resource utilization of multiple wastes and green cementitious materials. Background Art

[0002] At present, traditional methods of treating and disposing sludge, such as sanitary landfill, soil improvement and building material utilization, occupy a large area, consume a lot of energy, and easily cause secondary pollution to the environment and cause ecological and environmental problems.

[0003] Traditional sludge solidification requires dehydration first, and then the addition of composite solidification materials mainly composed of cement-based materials for solidification treatment. However, cement-based curing agents will release a large amount of carbon dioxide during the reaction process, which is increasingly inconsistent with the requirements of green construction and also has a high construction cost.

[0004] The amount of bulk solid waste added to the cementitious materials in the prior art is limited, and the binder is directly cement clinker. For example, the waste residue content of announcement number CN104909677B is only 68-75%, and the cement clinker content is 5-12%. The solid waste content of announcement number CN101215141B is less than 60%, and the cement content reaches 30-40%, and more than 30% of aggregate is used, and a variety of different alkaline activators and organic high molecular polymers are also used. The above-mentioned gel material has a low amount of bulk solid waste added, and still needs to add raw ore cement clinker binder and other additives, which does not meet the requirements of green environmental protection. Summary of the invention

[0005] The technical problem to be solved by the present application is to overcome the deficiencies and defects mentioned in the above background technology, solve the problem that the amount of bulk solid waste added to the gel material is low, and raw ore cement clinker binder and other additives still need to be added, and provide a method for preparing green cementitious material by synergistic resource utilization of multiple wastes, which has a bulk solid waste addition amount of more than 92.5%, does not require the addition of raw ore cement clinker binder, and has a high consolidation and stabilization effect on heavy metals and odors in sludge, and a green cementitious material.

[0006] In order to solve the above technical problems, the technical solution proposed in this application is:

[0007] A method for preparing green gelling materials by synergistic resource utilization of multiple wastes comprises the following preparation steps:

[0008] S1, grinding calcium-based waste slag to obtain active mineral powder;

[0009] S2, drying and dehydrating the desulfurized gypsum and grinding it to obtain desulfurized gypsum powder;

[0010] S3, mixing the calcium-based waste residue and the silicon-aluminum-based waste residue, calcining and grinding to obtain an active hydraulic gel;

[0011] S4, adding the desulfurized gypsum powder, the active hydraulic gel and the silicon-aluminum-based waste slag to the active mineral powder, and mixing and stirring to obtain a first mixture;

[0012] S5. Adding a first modifier and a second modifier into the first mixture, and performing rotational stirring to obtain a green gelling material.

[0013] In one embodiment, the active mineral powder in step S1 is a combination of one or more of slag, carbide slag and carbide furnace purification ash; the grinding time is 2 to 6 hours, and the particle size of the active mineral powder obtained after grinding is 100 to 1000 meshes.

[0014] In one embodiment, the drying conditions in step S2 are: a drying temperature of 130 to 180° C. and a drying time of 1 to 4 hours.

[0015] In one embodiment, after the desulfurized gypsum is dehydrated in step S2, the content of β-CaSO4·0.5H2O is ≥85%. Dehydration reaction: 2CaSO4·2H2O=2CaSO4·0.5H2O+3H2O, the main properties of the desulfurized gypsum after dehydration meet the following requirements: β-CaSO4·0.5H2O content ≥85%, standard consistency 60%, flexural strength ≥4.0MPa, compressive strength ≥6.0MPa, initial setting time 6-12min, final setting time 10-25min.

[0016] In one embodiment, the mass ratio of the calcium-based waste slag to the silicon-aluminum-based waste slag added in step S3 is 5-8:2-5, and the silicon-aluminum-based waste slag is a combination of one or more of steel slag, fly ash, and coal gasification slag.

[0017] In one embodiment, the calcination temperature in step S3 is 800-1200° C., the grinding time is 2-8 hours, and the particle size after grinding is 400-800 mesh.

[0018] In one embodiment, the mixing and stirring conditions in step S4 are: a mixing and stirring speed of 20 to 50 r / min, and a mixing and stirring time of 3 to 50 min.

[0019] In one embodiment, in step S5, the first modifier is naphthalene sulfonate, and the second modifier is a mixed modifier of one or more of montmorillonite powder, attapulgite, and sepiolite.

[0020] In one embodiment, the rotary stirring conditions in step S5 are: the rotary stirring speed is 100 to 120 r / min, and the rotary stirring time is 5 to 20 min.

[0021] Based on the overall inventive concept, the present application also provides a green gel material prepared by the above scheme, wherein the raw materials, measured by mass, include the following components: 30.0 to 50.0 parts of calcium-based active mineral powder, 10.0 to 20.0 parts of desulfurized gypsum, 10.0 to 20.0 parts of silicon-aluminum-based waste slag, 20.0 to 40.0 parts of active hydraulic gelling material, 1.0 to 2.0 parts of a first modifier and 3.0 to 6.0 parts of a second modifier.

[0022] Compared with the prior art, the beneficial effects of this application are:

[0023] 1. This application collaboratively utilizes a large amount of calcium-based waste slag, silicon-aluminum-based waste slag, etc., with the solid waste slag content reaching more than 92.5%, significantly reducing the emission of solid waste and reducing the pollution pressure on the environment. In terms of stimulating materials, the stimulating effect of solid waste desulfurization gypsum is used to "treat waste with waste", without the need to add additional chemical stimulants. It uses stirring for physical excitation, which is greener and more environmentally friendly and meets the needs of low-carbon sustainable development.

[0024] 2. The green cementitious material prepared by the preparation method of the present application has a good solidifying effect on soft soils such as silt to be solidified, and has a good solidifying and eliminating effect on heavy metals and odors in soft soils such as silt, and has obvious advantages over similar products. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 A schematic flow chart of the method for preparing green gelling materials by synergistic resource utilization of multiple wastes in the present application;

[0027] Figure 2 This is a graph showing the curing effect of the green gel material prepared in this application on heavy metal sludge cemented test blocks. DETAILED DESCRIPTION

[0028] To facilitate the understanding of the present application, the present application will be described in more comprehensive and detailed manner below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present application is not limited to the following specific embodiments.

[0029] Unless otherwise defined, all professional terms used below have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this application.

[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0031] The amount of dredging in urban rivers should not be underestimated, and water pollutants are easily accumulated and enriched in the sediment, and the mass concentration of pollutants such as nutrients, heavy metals and refractory organic matter (POPs) in the sediment is often much higher than the mass concentration of the corresponding pollutants in the overlying water. Therefore, the safe treatment and disposal of dredged sludge for various reasons (ensuring shipping safety, flood control and water environment protection, etc.) has received widespread attention from countries around the world, especially the safe disposal of sludge after dredging of polluted sediment has become a concern of water conservancy projects, municipal engineering and environmental engineering.

[0033] Since solidification / stabilization technology can improve the physical and mechanical properties of sludge (to facilitate subsequent resource utilization) and has a certain effect on solidifying and stabilizing pollutants (especially heavy metals and odors), the research on cementitious materials used for sludge solidification has become a hot topic at home and abroad.

[0034] Although there are many types of silt soft soil cementitious materials on the market, there is no product that can comprehensively achieve solidification in one go for some special silt soils, such as silt with serious excessive heavy metal content, foul odor, high organic matter content, and strong water stability.

[0035] At present, traditional methods of treating and disposing sludge, such as sanitary landfill, soil improvement and building material utilization, occupy a large area, consume a lot of energy, and easily cause secondary pollution to the environment and cause ecological and environmental problems. Traditional sludge solidification requires dehydration first, and then adding composite solidification materials mainly based on cement-based materials for solidification treatment, but cement-based solidifiers will release a large amount of carbon dioxide during the reaction process, and also have a high construction cost.

[0036] The amount of bulk solid waste added to the cementitious materials in the prior art is limited and the binder is directly made of cement clinker. The above-mentioned gel material has a low amount of bulk solid waste added and still needs to add raw ore cement clinker binder and other additives, which does not meet the requirements of green environmental protection.

[0037] In order to solve the above technical problems, the technical solution proposed in this application is:

[0038] A method for preparing green cementitious materials by synergistic resource utilization of multiple wastes, such as Figure 1As shown, the preparation steps include:

[0039] S1, grinding calcium-based waste slag to obtain active mineral powder;

[0040] S2, drying and dehydrating the desulfurized gypsum and grinding it to obtain desulfurized gypsum powder;

[0041] S3, mixing the calcium-based waste residue and the silicon-aluminum-based waste residue, calcining and grinding to obtain an active hydraulic gel;

[0042] S4, adding desulfurized gypsum powder, active hydraulic gelling material and silicon-aluminum-based waste residue to the active mineral powder, and mixing and stirring to obtain a first mixture;

[0043] S5. Add the first modifier and the second modifier to the first mixture, and perform rotation stirring to obtain a green gelling material.

[0044] The main component of desulfurized gypsum, β-CaSO4·0.5H2O, contributes greatly to the early strength of the system in the cementitious material system of this application due to its rapid hydration. At this time, mineral powder and fly ash mainly play a filling role. If the strength of the system is to be continuously improved in the later stage, the activity of mineral powder and fly ash must be better stimulated. The Si-O bond and Al-O bond energy in the mineral powder and fly ash system are large, and the glass structure in the mineral powder and fly ash has a high degree of polymerization, and the network connection is relatively tight. It is a mixture of three-dimensional continuous frame and layered structure, while the reaction of fly ash in the early cementitious system is only the reaction of Ca(OH)2 with soluble SiO2 and Al2O3. Under normal temperature and normal conditions, the depolymerization ability of mineral powder and fly ash is low and the depolymerization speed is slow. If the activity of mineral powder and fly ash is to be improved, the surface of mineral powder and fly ash must be cracked, the double electric layer protection structure composed of Si-O-Si and Si-O-Al must be destroyed, and the internal active SiO2 and Al2O3 must be continuously released. At the same time, the network structure of the gelling system with a high degree of polymerization must be continuously depolymerized to form monomers or dimers of silicon-oxygen tetrahedrons or aluminum-oxygen tetrahedrons. These depolymerized monomers or dimers will more easily react with Ca(OH)2 in the gelling system to generate hydrated calcium silicate and hydrated calcium aluminate. In order to better release the activity of mineral powder and fly ash, this application selects sulfate activators to stimulate the activity of mineral powder and fly ash. In order to maintain high early strength and mechanical properties, the basic mix ratio of the gelling material is selected as β-CaSO4·0.5H2O: silicon-aluminum-based waste slag = 2:1.

[0045] The first modifier, naphthalene sulfonate, is characterized by not only plasticity for sludge solidification, but also greatly reducing harmful pores and significantly enhancing compressive strength. The second modifier selects clay-modified mineral powders such as montmorillonite powder, attapulgite, and sepiolite, which can adsorb heavy metals in sludge soil, lock heavy metals without leaching, meet environmental quality standards, and have a good effect on eliminating sludge odor. The surface and end faces of the clay-modified mineral powder modifier are rich in polyhydroxy structures, and the amount of hydroxyl groups between the layers will increase after inorganic modification. Heavy metal ions can be complexed with these hydroxyl structures. In addition, there are convertible cations in the interlayer domain of the original soil of the clay-modified mineral powder modifier, and heavy metal ions can exchange these cations to enter the interlayer. There are fewer exchangeable cations between the layers of the clay-modified mineral powder modifier, but because the interlayer domain is stretched, heavy metal ions can diffuse into its interlayer and complex with surface groups. A large number of hydroxyl groups are exposed on the surface and end faces of the clay-modified mineral powder modifier and the inorganic modified product, while fulvic acid is mainly aromatic and contains a large number of functional group structures such as hydroxyl (-OH), carboxyl (-COOH), and carbonyl (-C=O). These functional groups help fulvic acid to complex and adsorb with the polyhydroxyl structure of the adsorbent, so that fulvic acid is fixed on it. Due to the diversity of functional groups on fulvic acid, its complexation mode with the surface and end face hydroxyl groups of the clay-modified mineral powder modifier and the inorganic modified product is different, and there may be multiple complexation modes. Fulvic acid adsorbed on the surface of clay-modified mineral powder modifier or oxide can significantly improve the physical and chemical properties of the surface of clay-modified mineral powder modifier or oxide. Some potential properties can be determined by the fulvic acid attached to the surface, and the clay-modified mineral powder modifier attached with fulvic acid is easier to complex with heavy metal ions, which enhances the ability of the clay-modified mineral powder modifier to complex with metal ions. The clay-modified mineral powder modifier has high porosity and extremely strong gas adsorption capacity, which can effectively adsorb malodorous gases.

[0046] This application makes collaborative resource utilization of a large amount of calcium-based waste residue, silicon-aluminum-based waste residue, etc., with the solid waste residue dosage reaching more than 92.5%, significantly reducing the discharge of solid waste and reducing the pollution pressure on the environment. In terms of stimulating materials, the stimulating effect of solid waste desulfurization gypsum is used to "use waste to treat waste", without the need to add additional chemical stimulants, and the method of physical stimulation by stirring is more green and environmentally friendly, in line with the needs of low-carbon sustainable development. The green cementitious material prepared by the preparation method of this application has a good solidification effect on soft soils such as silt to be solidified, and has a good solidification and elimination effect on heavy metals and odors in soft soils such as silt, which has obvious advantages over similar products.

[0047] The technical solution of the present application is illustrated below by means of specific embodiments.

[0048] Embodiment 1:

[0049] A green cementitious material is prepared by synergistic resource utilization of multiple wastes, and its raw material components include: 340g of active mineral powder activated by physical grinding of calcium-based waste slag and water slag, 200g of desulfurized gypsum calcined at high temperature, 60g of fly ash, 40g of coal gasification slag, 300g of active hydraulic cementitious material, 10g of naphthalene sulfonate modifier, 30g of montmorillonite powder modifier, and 20g of attapulgite.

[0050] Prepared using the following steps:

[0051] A. Grind the calcium-based waste residue for 3-5 hours to obtain 400 g of active mineral powder;

[0052] B. The desulfurized gypsum is placed in an oven at 180°C for 2 hours and then ground for 2-4 hours to activate its activity for later use;

[0053] C. Calcium-based waste residue and silicon-aluminum-based waste residue are mixed in a mass ratio of 8:2, calcined and ground for 6-8 hours to obtain an active hydraulic gel, which is ready for use;

[0054] D. Add 200 g of desulfurized gypsum, 100 g of silicon-aluminum-based waste slag and 300 g of active hydraulic gel respectively to 400 g of active mineral powder, and stir rapidly at 50 r / min to obtain a first mixture for 15 min;

[0055] E. Add 10 g of the first modifier and 50 g of the second modifier to the first mixture respectively, and stir again at a high speed of 120 r / min for 20 min to fully activate the activity, thereby obtaining a green gelling material prepared by synergistic resource utilization of multiple wastes.

[0056] Conduct heavy metal sludge solidification performance test:

[0057] (1) Take sludge from a certain channel and test its moisture content by drying method. According to the moisture content of sludge and the required compressive strength after 28 days, determine the proportion of cementitious material to be added.

[0058] (2) According to the determined cementitious material incorporation ratio, the cementitious material is mixed into the sludge and stirred evenly.

[0059] (3) The evenly mixed solidified soil is molded into a 70.7*70.7*70.7mm plastic triple mold and continuously vibrated to ensure that the air in the solidified soil is discharged and the filling is dense.

[0060] (4) After the mold is installed, place it in a standard curing room at a temperature of 23±2℃ and a humidity of 90±2% for 7d, 14d, and 28d respectively. Test the unconfined compressive strength at 7d, 14d, and 28d respectively.

[0061] In this embodiment, the cementitious test block was prepared according to the weight ratio of green cementitious material to sludge = 1:8. Figure 2 As shown:

[0062] The unconfined compressive strength at 7d, 14d and 28d was tested to be 1.48MPa, 2.16MPa and 3.05MPa respectively. The early strength increased significantly, and the strength after 28 days reached the 3.0 strength grade of soft soil solidifier CJ / T 526-2018.

[0063] After curing in a standard curing room at 23±2℃ and 90±2% humidity for 7 days, the steel was placed in tap water for 7 days, 14 days and 28 days, and the water stability strength was tested to be 1.21MPa, 2.29MPa and 3.13MPa respectively. The strength increased slightly after 28 days of immersion, and the water stability met the application technical requirements.

[0064] The sludge in this example has a serious excess of cadmium. After 28 days of curing, the sludge cement test block was tested by a third party for heavy metal water immersion, as shown in Table 1:

[0065] Table 1 Heavy metal water leaching test results of heavy metal sludge cement test blocks in a certain channel

[0066]

[0067] According to the heavy metal water leaching test results in Table 1 above, they all meet the basic item standard limits of surface water environmental quality standard GB 3838-2002.

[0068] Embodiment 2:

[0069] A green cementitious material is prepared by synergistic resource utilization of multiple wastes, and its raw material components include: 310g of active mineral powder after physical grinding and activation of calcium-based waste slag and water slag, 100g of calcium carbide slag powder, 150g of high-temperature calcined desulfurized gypsum, 90g of coal gasification slag, 50g of tailings, 220g of active hydraulic cementitious material, 20g of naphthalene sulfonate as a modifier, and 60g of montmorillonite powder as a modifier. The green cementitious material is prepared according to the process steps of Example 1.

[0070] Performance test after soft soil solidification test on slope bank:

[0071] According to the moisture content of soft soil and the required 28-day compressive strength, the cementitious material mixing ratio is determined to be 1:8. According to the determined cementitious material mixing ratio, the cementitious material is mixed into the soft soil, the soft soil particle size is ≦1.0cm, and stirred evenly, and water is sprayed appropriately. The mixed solidified soil is molded into a 70.7*70.7*70.7mm steel triple mold and compacted. After the mold is completed, it is placed in a standard curing room at a temperature of 23±2℃ and a humidity of 90±2% for 7d, 14d, and 28d respectively.

[0072] The unconfined compressive strength at 7d, 14d and 28d of testing were 2.52MPa, 4.13MPa and 5.89MPa respectively. The strength increased rapidly in the early stage and steadily in the later stage. The 7-day strength reached the requirements of JTGE51 of Test Code for Stabilized Materials of Inorganic Binders for Highway Engineering.

[0073] After curing in a standard curing room at 23±2℃ and 90±2% for 7 days, the water-stable strength was tested to be 6.15MPa after being immersed in tap water for 28 days. The strength increased after immersion for 28 days, and the water stability met the application technical requirements.

[0074] Embodiment 3:

[0075] A green cementitious material prepared by synergistic resource utilization of multiple wastes, the raw material components of which include: 380g of active mineral powder calcium-based waste slag carbide slag powder after physical grinding and excitation, 100g of carbide furnace purified ash, 100g of high-temperature calcined desulfurized gypsum, 50g of silicon-aluminum-based waste fly ash, 55g of coal gasification slag, 50g of tailings, 200g of active hydraulic cementitious material, 15g of modifier naphthalene sulfonate, 25g of modifier attapulgite, 10g of sepiolite, and 15g of montmorillonite powder. The green cementitious material is prepared according to the process steps of Example 1.

[0076] Performance test of malodorous sludge after solidification:

[0077] (1) Take sludge from a certain channel and test its moisture content by drying method. According to the moisture content of sludge and the required compressive strength after 28 days, determine the proportion of cementitious material to be added.

[0078] (2) According to the determined cementitious material incorporation ratio, the cementitious material is mixed into the sludge and stirred evenly.

[0079] (3) The evenly mixed solidified soil is molded into a 70.7*70.7*70.7mm plastic triple mold and continuously vibrated to ensure that the air in the solidified soil is discharged and the filling is dense.

[0080] (4) After the mold is installed, place it in a standard curing room at a temperature of 23±2℃ and a humidity of 90±2% for 7d, 14d, and 28d respectively. Test the unconfined compressive strength at 7d, 14d, and 28d respectively.

[0081] In this embodiment, cementitious test blocks were prepared according to the weight ratio of cementitious material to sludge = 1:8. The unconfined compressive strengths at 7d, 14d, and 28d were 1.25MPa, 1.53MPa, and 2.3MPa, respectively. The strength at 28 days reached the 2.0 strength grade of soft soil solidifier CJ / T 526-2018.

[0082] After curing in a standard curing room at 23±2℃ and 90±2% for 7 days, the steel was placed in tap water for 7 days, 14 days and 28 days, and the water stability strength was tested to be 1.39MPa, 1.91MPa and 2.5MPa respectively. The strength increased slightly after 28 days of immersion, and the water stability met the application technical requirements.

[0083] When the foul-smelling sludge is completely solidified, the foul smell will completely disappear, which not only satisfies the requirement of in-situ solidification of the sludge, avoids transportation and secondary pollution, but also solves the problem of foul smell emitted from the river.

[0084] In summary, it can be seen from the test results of Examples 1, 2 and 3 that the green cementitious material for comprehensive utilization of multiple wastes provided by the present application has obvious environmental restoration and improvement for the silt soil to be solidified, especially including but not limited to high content of heavy metals, odor, and in-situ solidification of silt soil to avoid secondary pollution and transportation, compared with ordinary curing agents.

[0085] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0086] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing green cementitious materials by synergistic resource utilization of multiple wastes, characterized in that: include: S1, grinding calcium-based waste slag to obtain active mineral powder; S2, drying and dehydrating the desulfurized gypsum and grinding it to obtain desulfurized gypsum powder; S3, mixing the calcium-based waste residue and the silicon-aluminum-based waste residue, calcining and grinding to obtain an active hydraulic gel; S4, adding the desulfurized gypsum powder, the active hydraulic gel and the silicon-aluminum-based waste slag to the active mineral powder, and mixing and stirring to obtain a first mixture; S5. Adding a first modifier and a second modifier into the first mixture, and performing rotational stirring to obtain a green gelling material.

2. The method according to claim 1, characterized in that The active mineral powder in step S1 is a combination of one or more of water slag, carbide slag and carbide furnace purification ash; the grinding time is 2 to 6 hours, and the particle size of the active mineral powder obtained after grinding is 100 to 1000 meshes.

3. The method according to claim 1, characterized in that The drying conditions in step S2 are as follows: the drying temperature is 130-180° C. and the drying time is 1-4 hours.

4. The method according to claim 1, characterized in that: After the desulfurized gypsum is dehydrated in step S2, the content of β-CaSO4·0.5H2O is ≥85%.

5. The method according to claim 1, characterized in that: In step S3, the mass ratio of the added amount of the calcium-based waste slag to the silicon-aluminum-based waste slag is 5-8:2-5, and the silicon-aluminum-based waste slag is a combination of one or more of steel slag, fly ash, and coal gasification slag.

6. The method according to claim 1, characterized in that The calcination temperature in step S3 is 800-1200° C., the grinding time is 2-8 hours, and the particle size after grinding is 400-800 meshes.

7. The method according to claim 1, characterized in that The mixing and stirring conditions in step S4 are: a mixing and stirring speed of 20 to 50 r / min, and a mixing and stirring time of 3 to 50 min.

8. The method according to claim 1, characterized in that In step S5, the first modifier is naphthalene sulfonate, and the second modifier is a mixed modifier of one or more of montmorillonite powder, attapulgite, and sepiolite.

9. The method according to claim 1, characterized in that: The rotary stirring conditions in step S5 are: a rotary stirring speed of 100 to 120 r / min, and a rotary stirring time of 5 to 20 min.

10. A green gel material prepared by the method according to any one of claims 1 to 9, characterized in that: The raw materials include the following components by mass: 30.0-50.0 parts of calcium-based active mineral powder, 10.0-20.0 parts of desulfurized gypsum, 10.0-20.0 parts of silicon-aluminum-based waste slag, 20.0-40.0 parts of active hydraulic gelling material, 1.0-2.0 parts of a first modifier and 3.0-6.0 parts of a second modifier.