Mineralization rust-inhibiting auxiliary agent for carbon sequestration concrete
By using mineralizers such as calcium carbonate, calcium silicate and calcium hydroxide, rust inhibitors such as sodium chromate, sodium molybdate and sodium zincate in concrete, as well as catalysts, the internal environment of the concrete is improved, and CO2 diffusion and reinforcement are solved. The problem of corrosion protection improves carbon sequestration and rust resistance.
Patent Information
- Application Number
- CN202411177376.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
During the CO2 mineralization and curing concrete process, the generated stable carbonate accumulates on the surface, hindering the spread of CO2, reducing the carbon sequestration rate, and leading to premature corrosion of the steel bars.
Use a composite additive including mineralizers, rust inhibitors and catalysts. The mineralizer consists of calcium carbonate, calcium silicate and calcium hydroxide. The rust inhibitor consists of sodium chromate, sodium molybdate and sodium zincate. The catalyst is It consists of maleic acid, distilled water and potassium hydroxide solution. By improving the alkaline environment and structure of the concrete, it promotes CO2 diffusion and steel bar corrosion protection.
It significantly improves the carbon sequestration rate and mechanical properties of concrete, and provides good rust resistance properties to prevent premature rust of steel bars, solving the problems of low carbon sequestration rate and rust during mineralization and maintenance.
Smart Images

Figure BDA0005011073760000111 
Figure BDA0005011073760000121 
Figure BDA0005011073760000131
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building material processing, and in particular to a mineralized rust-inhibiting additive for carbon-fixing concrete. Background Art
[0002] Carbon Capture, Utilization and Storage (CCUS) refers to separating and purifying CO2 from industrial or related energy sources, and then recycling it into new production processes. This can not only reduce carbon emissions, but also generate economic benefits, so it is more practical. After years of development, CCUS technology has been accepted and used worldwide.
[0003] The application of CCUS technology in the construction industry is reflected in the use of CO2 mineralization to cure concrete. When CO2 reacts with Ca in cement, 2 + and Mg 2+ The reaction generates CaCO3 and MgCO3, which are permanently solidified into the concrete. It can also shorten the initial setting time of the concrete, improve the compressive strength and reduce the amount of cement. However, during the mineralization curing process, due to the mineralization reaction, the stable carbonate generated will accumulate on the surface of the concrete, hindering the diffusion of CO2 into the interior of the concrete, thereby reducing the carbon fixation rate of the concrete and resulting in unsatisfactory mineralization curing effects. At the same time, after mineralization curing, the pH value inside the reinforced concrete will be reduced, causing the internal steel bars to rust prematurely. Summary of the invention
[0004] In order to solve the problem that the carbon fixation rate of concrete is easily reduced and rusts prematurely during the mineralization and curing process, the present invention discloses a mineralization rust-inhibiting additive for carbon-fixing concrete, including a mineralizer, a rust inhibitor and a catalyst, which can effectively improve the carbon fixation rate of concrete and the corresponding mechanical properties, and also make the concrete have good rust-inhibiting performance.
[0005] The specific technical scheme of the present invention is:
[0006] First, the present invention discloses a mineralized rust-inhibiting additive for carbon-fixing concrete, comprising a mineralizer, a rust-inhibiting agent and a catalyst, wherein the mineralizer comprises at least one of calcium carbonate, calcium silicate and calcium hydroxide;
[0007] The rust inhibitor includes at least one of sodium chromate, sodium molybdate and sodium zincate.
[0008] During the mineralization curing process of concrete, due to the mineralization reaction, the generated stable carbonate will accumulate on the surface of the concrete, hindering the diffusion of CO2 into the interior of the concrete, thereby reducing the carbon fixation rate of the concrete and resulting in unsatisfactory mineralization curing effect; at the same time, after the mineralization curing, the internal pH of the reinforced concrete components will be reduced, resulting in premature corrosion of the internal steel bars. The inventors of the present application have noticed that adding the above-mentioned mineralizer to ordinary silicate concrete has the following effects: (1) It is determined through microscopic characterization that limestone powder with a maximum particle size of 20 μm can be used as a crystallization point for the precipitation of the reaction product calcium carbonate, and induce calcium silicate (C3S and C2S) in silicate concrete to participate in the reaction; (2) The amorphous calcium silicate doped in the concrete can not only react with CO2, but also increase the mineralization rate and amount of silicate concrete. The silicate doping as a dispersant strengthens the internal diffusion of CO2 gas, especially the gas permeability in the early stage of the reaction; (3) The alkalinity of calcium hydroxide helps to accelerate the carbonation reaction in concrete. In addition, the water and carbon dioxide in the concrete are more likely to form calcium carbonate under the action of calcium hydroxide, which can increase the rate and efficiency of carbonization. In addition, calcium hydroxide has a high alkalinity. When it dissolves in concrete and releases calcium hydroxide ions (OH-), it can increase the alkaline environment of the concrete. The corrosion of steel bars generally occurs in an acidic environment because the acidic environment can accelerate the corrosion reaction on the surface of the steel bars. By increasing the alkalinity of concrete, the acidic environment inside the concrete can be reduced, thereby slowing down the corrosion rate of the steel bars.
[0009] At the same time, the anodic rust inhibitor improves the passive film of the steel bar to reduce the contact between the steel bar and oxygen, thereby preventing the corrosion of the steel bar; the cathodic rust inhibitor improves the corrosion resistance of the steel bar by forming an adsorption film layer on the surface of the steel bar; the composite rust inhibitor provided by the present invention (including the anodic rust inhibitors sodium chromate and sodium molybdate, and the cathodic rust inhibitor sodium zincate) overcomes the shortcomings of a single type of rust inhibitor and has the characteristics of both anodic and cathodic rust inhibitors.
[0010] The above catalysts have a great influence on Ca 2+ It has a very high binding capacity and forms calcium complexes that migrate quickly in concrete and migrate to larger pores and cracks. The calcium complexes in the pores and cracks combine with CO3 2- 、SiO3 2- It reacts to generate crystal precipitates such as CaCO3 and CaSiO3, which further optimizes the pore structure of the concrete and promotes the mineralization reaction. After the reaction, it returns to its original state and realizes the function of repeated use.
[0011] In a possible implementation, the mineralizer comprises 75 to 90 parts, the rust inhibitor comprises 7 to 20 parts, and the catalyst comprises 3 to 5 parts by weight.
[0012] In a possible implementation, the catalyst includes: maleic acid, distilled water, potassium hydroxide solution and hydrogen peroxide solution.
[0013] In a possible implementation, the catalyst is composed of maleic acid, distilled water, potassium hydroxide solution and hydrogen peroxide solution in a weight ratio of 1:1:1:0.3, and the concentration of the potassium hydroxide solution is 0.15 mol / L, and the mass fraction of the hydrogen peroxide solution is 30%.
[0014] In a possible implementation, the catalyst is prepared by weighing sodium hydroxide powder to prepare a 0.15 mol / L solution for use, then weighing maleic acid and distilled water, mixing the two, placing them in a water bath heating environment and stirring, and when all are dissolved, adding the prepared sodium hydroxide solution and potassium hydroxide solution in proportion, stirring for 1 minute, stopping heating, and obtaining the catalyst.
[0015] In a possible implementation, the mineralizer consists of two of calcium carbonate, calcium silicate and calcium hydroxide, wherein the weight ratio of the calcium carbonate to the calcium silicate is 1:1, or the weight ratio of the calcium carbonate to the calcium hydroxide is 4:1, or the weight ratio of the calcium silicate to the calcium hydroxide is 4:1.
[0016] In a possible implementation, the mineralizer consists of calcium carbonate, calcium silicate and calcium hydroxide, wherein the weight ratio of the calcium carbonate, calcium silicate and calcium hydroxide is 2:2:1.
[0017] In a possible implementation, the rust inhibitor is composed of two of sodium chromate, sodium molybdate and sodium zincate, wherein the weight ratio of the sodium chromate to the sodium molybdate is 1:1, or the weight ratio of the sodium chromate to the sodium octanoate is 1:1, or the weight ratio of the sodium molybdate to the sodium octanoate is 1:1.
[0018] The inventors of the present application accidentally discovered in experiments that adding corresponding mineralizers, rust inhibitors and catalysts according to the above weight ratio can make concrete have a higher carbon fixation rate, better mechanical properties and better rust resistance.
[0019] Second, the present invention also provides a method for using the above-mentioned mineralized rust inhibitor, comprising: mixing and grinding the mineralizer and the rust inhibitor in proportion, adding them into the concrete slurry together with the catalyst, and continuously stirring the concrete slurry during the adding process.
[0020] In a possible implementation, the mineralized rust-inhibiting agent added to the concrete slurry accounts for 10-14% of the weight of the cement in the concrete slurry. The inventors of the present application have found in experiments that when the mineralized rust-inhibiting agent is added in the above proportion, the carbon fixation rate, mechanical properties and rust-inhibiting properties of the concrete can be better.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] (1) After CO2 mineralization curing, the carbon fixation rate, durability and mechanical properties of concrete with mineralization additives can be effectively improved; at the same time, the concrete has good rust resistance. This solves the problems of low carbon fixation rate and premature rust of steel bars during the mineralization curing process.
[0023] (2) The mixed use of mineralizers can improve the carbon fixation effect in many ways. For example, the addition of calcium carbonate can provide crystallization points for the products generated by the mineralization reaction; the introduction of calcium silicate can enhance the diffusion capacity of carbon dioxide in the pores inside the concrete; the addition of calcium hydroxide not only provides an alkaline environment for the mineralization reaction, but also participates in the mineralization process as a reactant. The combined use of three mineral additives with different properties can effectively exert their respective performance advantages.
[0024] (3) The mixture of mineralizer, rust inhibitor and catalyst can produce synergistic effect. Under the joint action of mineralizer and catalyst, the surface layer of concrete becomes denser, reducing the intrusion of external water and oxygen, thereby cooperating with rust inhibitor to better prevent steel corrosion; and under the action of rust inhibitor, the steel bars inside the concrete will not rust prematurely, thus not hindering the smooth progress of mineralization reaction. DETAILED DESCRIPTION
[0025] Examples of the present embodiment are described in detail below. The examples are only used to explain the present embodiment and are not to be construed as limiting the present embodiment.
[0026] In the description of the embodiments of the present application, it should be noted that all ranges disclosed in the present application will be understood to include any and all sub-ranges included therein. For example, the stated range "3% to 20%" should be deemed to include any and all sub-ranges as follows: it starts with a minimum value of 3% or greater and ends with a maximum value of 20% or less, for example, 4% to 19%, or 4.5% to 15%, or 12% to 13%. At the same time, all ranges disclosed in the present application are also deemed to include the endpoints of the ranges, unless otherwise explicitly stated. For example, the range "between 4 and 6" or "4 to 6" or "4-6" should generally be deemed to include endpoints 4 and 6.
[0027] In the description of this embodiment, "several" means one or more, "more" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0028] In this application, the term "carbon sequestration" refers to a governance approach to reduce the concentration of carbon dioxide in the atmosphere. It is one of the carbon neutrality technical paths, mainly including three aspects: carbon capture and storage, carbon capture and energy utilization, and carbon capture and resource utilization. In this application, the term "mineralization" mainly refers to CO2 mineralization, which refers to the use of bulk solid waste rich in calcium and magnesium (such as steelmaking slag, cement kiln dust, fly ash, phosphogypsum, etc.) to mineralize CO2 and produce chemical products, while achieving CO2 emission reductions and obtaining inorganic chemical products with certain value, so as to treat waste with waste and improve the economic efficiency of resource utilization of CO2 and solid waste.
[0029] Unless otherwise specified, the terms used herein have the same meaning as commonly understood by those skilled in the art. If a term is defined herein and its definition is different from the commonly understood meaning in the art, the definition herein shall prevail.
[0030] In the first aspect, the present application provides a mineralized rust-inhibiting agent for carbon-fixing concrete, including a mineralizer, a rust inhibitor and a catalyst. It can be understood that in addition to the above-mentioned raw materials, the mineralized rust-inhibiting agent can also contain other additives that can enhance or improve a certain function of concrete.
[0031] In some possible embodiments, the mineralizer includes at least one of calcium carbonate, calcium silicate and calcium hydroxide. It is understood that the mineralizer can be composed of calcium carbonate, calcium silicate or calcium hydroxide alone, or calcium carbonate and calcium silicate, or calcium carbonate and calcium hydroxide, or calcium silicate and calcium hydroxide, or calcium carbonate, calcium silicate and calcium hydroxide together. In some possible embodiments, the mineralizer is composed of two of calcium carbonate, calcium silicate and calcium hydroxide. In some preferred embodiments, the weight ratio of calcium carbonate to calcium silicate is about 1:2 to 2:1, or the weight ratio of calcium carbonate to calcium hydroxide is about 3:1 to 5:1, or the weight ratio of calcium silicate to calcium hydroxide is about 2:1 to 5:1. In some more preferred embodiments, the weight ratio of calcium carbonate to calcium silicate is 1:1, or the weight ratio of calcium carbonate to calcium hydroxide is 4:1, or the weight ratio of calcium silicate to calcium hydroxide is 4:1. In some possible embodiments, the mineralizer consists of calcium carbonate, calcium silicate and calcium hydroxide. In some preferred embodiments, the weight ratio of calcium carbonate, calcium silicate and calcium hydroxide is 2:2:1.
[0032] In some possible embodiments, the rust inhibitor includes: at least one of sodium chromate, sodium molybdate and sodium zincate. It is understandable that the rust inhibitor is composed of sodium chromate, sodium molybdate and sodium zincate, or is composed of sodium chromate and sodium molybdate, or is composed of sodium chromate and sodium zincate, or is composed of sodium molybdate and sodium zincate, or is sodium chromate, or is sodium molybdate, or is sodium zincate. In some preferred embodiments, the rust inhibitor is composed of two of sodium chromate, sodium molybdate and sodium zincate. In some more preferred embodiments, the weight ratio of the sodium chromate to the sodium molybdate is 1:1, or the weight ratio of the sodium chromate to the sodium octanoate is 1:1, or the weight ratio of the sodium molybdate to the sodium octanoate is 1:1.
[0033] In some possible embodiments, the catalyst includes: maleic acid, distilled water, potassium hydroxide solution and hydrogen peroxide solution. In some preferred embodiments, the catalyst is composed of maleic acid, distilled water, potassium hydroxide solution and hydrogen peroxide solution in a weight ratio of 1:1:1:0.3. More preferably, the concentration of the potassium hydroxide solution is 0.15 mol / L and the mass fraction of the hydrogen peroxide solution is 30%. In some possible embodiments, the preparation method of the catalyst is: weigh sodium hydroxide powder, prepare a 0.15 mol / L solution for standby use, then weigh maleic acid and distilled water, mix the two, place them in a water bath heating environment and stir, and when they are completely dissolved, add the prepared sodium hydroxide solution and potassium hydroxide solution in proportion, stir for 1 minute, stop heating, and obtain the catalyst.
[0034] In a second aspect, the present invention provides a method for using the above-mentioned mineralized rust inhibitor. In some possible embodiments, the method comprises: mixing and grinding the mineralizer and the rust inhibitor in proportion. In some possible embodiments, the mineralizer is 75 to 90 parts, the rust inhibitor is 7 to 20 parts, and 3 to 5 parts of the catalyst are added to the concrete slurry together, and stirring is continued during the addition process. In some preferred embodiments, the mineralized rust inhibitor added to the concrete slurry accounts for 10 to 14% of the weight of the cement in the concrete slurry.
[0035] The technical solution of the present application is further explained and illustrated by way of examples and comparative examples.
[0036] Example 1
[0037] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0038] Example 2
[0039] Example 2 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 30 parts of calcium carbonate, 30 parts of calcium silicate, 15 parts of calcium hydroxide, 20 parts of sodium chromate, and 5 parts of catalyst.
[0040] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0041] Example 3
[0042] Example 3 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 37.5 parts of calcium carbonate, 37.5 parts of calcium silicate, 10 parts of sodium chromate, 10 parts of sodium zincate, and 5 parts of a catalyst.
[0043] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0044] Example 4
[0045] Example 4 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 60 parts of calcium carbonate, 15 parts of calcium hydroxide, 10 parts of sodium chromate, 10 parts of sodium molybdate, and 5 parts of a catalyst.
[0046] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0047] Example 5
[0048] Example 5 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 60 parts of calcium carbonate, 15 parts of calcium hydroxide, 20 parts of sodium chromate, and 5 parts of catalyst.
[0049] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0050] Example 6
[0051] Example 6 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 60 parts of calcium silicate, 15 parts of calcium hydroxide, 20 parts of sodium zincate, and 5 parts of catalyst.
[0052] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0053] Example 7
[0054] Example 7 provides a mineralization aid, which is composed of the following raw materials, in parts by weight: 36 parts of calcium carbonate, 36 parts of calcium silicate, 18 parts of calcium hydroxide, 3.5 parts of sodium chromate, 3.5 parts of sodium zincate, and 3 parts of a catalyst.
[0055] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0056] Example 8
[0057] Example 8 provides a mineralization aid, which is composed of the following raw materials, in parts by weight: 36 parts of calcium carbonate, 36 parts of calcium silicate, 18 parts of calcium hydroxide, 7 parts of sodium chromate, and 3 parts of catalyst.
[0058] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0059] Example 9
[0060] Example 9 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 45 parts of calcium carbonate, 45 parts of calcium silicate, 3.5 parts of sodium chromate, 3.5 parts of sodium zincate, and 3 parts of catalyst.
[0061] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0062] Example 10
[0063] Example 10 provides a mineralization aid, which is composed of the following raw materials, in parts by weight: 72 parts of calcium carbonate, 18 parts of calcium hydroxide, 3.5 parts of sodium chromate, 3.5 parts of sodium molybdate, and 3 parts of a catalyst.
[0064] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0065] Embodiment 11
[0066] Example 11 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 78 parts of calcium carbonate, 12 parts of calcium hydroxide, 7 parts of sodium chromate, and 3 parts of catalyst.
[0067] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0068] Example 12
[0069] Example 12 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 78 parts of calcium silicate, 12 parts of calcium hydroxide, 7 parts of sodium zincate, and 3 parts of catalyst.
[0070] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0071] Comparative Example 1
[0072] Comparative Example 1 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 75 parts of calcium carbonate, 20 parts of sodium zincate, and 5 parts of catalyst.
[0073] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0074] Comparative Example 2
[0075] Comparative Example 2 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 75 parts of calcium silicate, 20 parts of sodium chromate, and 5 parts of catalyst.
[0076] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 14%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0077] Comparative Example 3
[0078] Comparative Example 3 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 90 parts of calcium carbonate, 7 parts of sodium zincate, and 3 parts of catalyst.
[0079] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0080] Comparative Example 4
[0081] Comparative Example 4 provides a mineralization aid, which is composed of the following raw materials in parts by weight: 90 parts of calcium silicate, 7 parts of sodium chromate, and 3 parts of catalyst.
[0082] The above-mentioned mineralization additive was added to C35 concrete at a dosage of 9%; a test specimen with a size of 150mm×150mm×150mm was cast, and after the concrete specimen was demoulded and pre-cured for 5 hours (wind speed of 1m / s, temperature of 25°C, relative humidity of 50%), it was placed in a reactor for mineralization curing for 4 hours (temperature of 45°C, carbon dioxide concentration of 99%, curing pressure of 0.5MPa, humidity of 60%). After the mineralization curing was completed, some of the specimens were taken out for carbon fixation rate testing, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the concrete specimen compressive strength test was carried out.
[0083] At the same time, in order to reflect the effects of each concrete mineralization additive provided by the present invention, C35 concrete was mineralized and cured as a blank control example. The mineralization additive provided by the present invention was not added to the blank control example. After the mineralization and curing were completed, some specimens were taken out for carbon fixation rate test, and the remaining specimens were taken out and placed in a standard curing room (temperature of 20±2°C, humidity of more than 95%), cured for 28 days, and then the compressive strength test of the concrete specimens was carried out.
[0084] Table 1 shows the mix ratio standard of C35 concrete in the above-mentioned embodiment and comparative example. The parameter comparison of the above-mentioned embodiment and comparative example is shown in Table 2.
[0085] Table 1
[0086]
[0087] Table 2
[0088]
[0089] Performance Evaluation
[0090] In the above concrete forming process, the treated steel bars are embedded in the concrete and connected by wires. After the concrete specimen is demoulded and pre-cured for 5 hours (wind speed is 1m / s, temperature is 25℃, relative humidity is 50%), it is placed in a reactor for mineralization curing for 4 hours (temperature is 45℃, carbon dioxide concentration is 99%, curing pressure is 0.5MPa, humidity is 60%), and then placed in a standard curing room (temperature is 20±2℃, humidity is above 95%) for 28 days, and then soaked in a 3% NaCl solution for three months. After three months, the corrosion potential and corrosion current density of the steel bars are tested by an electrochemical workstation, and the corrosion condition of the steel bars in the concrete is judged according to the evaluation criteria in GB / T338032017 "Technical Specifications for the Application of Corrosion Inhibitors for Reinforced Concrete".
[0091] The compressive strength of concrete cube test blocks is tested with reference to GB / T 50081-2019 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", and an electrochemical comprehensive evaluation test is carried out in accordance with GB / T33803-2017 "Technical Specifications for the Application of Corrosion Inhibitors in Reinforced Concrete", and the corrosion condition of the steel bars in the concrete is evaluated. It is generally believed that when the corrosion potential is greater than -200mV, the steel bars have no corrosion activity or the corrosion activity is uncertain, and the probability of corrosion is 5%; when the corrosion potential is in the range of -200mV to -350mV, the probability of steel bars corroding is 50%; when the corrosion potential is in the range of -350mV to -500mV, the probability of steel bars corroding is 95%. Similarly, the corrosion state of the steel bars can be judged according to the size of the apparent corrosion current density: when the apparent corrosion current density is less than 0.2μA / cm 2 When the apparent corrosion current density is 0.2μA / cm 2 ~0.5μA / cm 2 When the apparent corrosion current density is 0.5μA / cm 2 ~1.0μA / cm 2 When the apparent corrosion current density is greater than 1.0 μA / cm 2 When the steel bar is at a high corrosion rate, the corrosion state of the steel bar can be used to determine the anti-rust effect of the admixture.
[0092] The carbon fixation rate is calculated by the weight gain method-drying to absolute dryness method. The principle is that the water evaporated during the mineralization reaction comes from the free water in the specimen. Therefore, the mass reduction of the specimen after drying to constant weight at (105±5)℃ can be used to approximate the mass of free water in the specimen, and the amount of evaporated water can be estimated by the difference in the free water content in the specimen before and after curing, thereby compensating for the carbon fixation obtained by the direct weight gain method.
[0093]
[0094] In the actual operation, since complete drying has an impact on the curing process of the specimens, specimens A and B of the same batch are dried before and after curing to determine the moisture content before and after curing. Specimen A before curing is placed in an oven at (105±5)℃ and dried to constant weight. The drying mass loss Δm A-drying The mass fraction of specimen A before curing is recorded as free water content δ before ; Take another specimen B and record the mass before and after mineralization curing, m B-before and m B-after , place the cured specimen B in an oven at (105±5)℃ and dry it to constant weight, and set the drying mass loss Δm B-drying The mass fraction of specimen B after curing is recorded as free water content δ after .
[0095] In summary, the calculation formula for carbon fixation rate (based on the weight of cement dry material) is:
[0096]
[0097] The test results are shown in Table 3.
[0098] Table 3
[0099]
[0100] According to Table 2 and Table 3, by comparing Example 1 and Example 2, it can be seen that when the rust inhibitor is two of sodium chromate, sodium molybdate and sodium zincate and the weight ratio is 1:1, the concrete has better performance in compressive strength, carbon fixation rate and rust inhibition performance;
[0101] By comparing Example 1, Example 3 and Comparative Example 1, Comparative Example 2, it can be seen that when the mineralizer is composed of calcium carbonate, calcium silicate and calcium hydroxide in a weight ratio of 2:2:1, the concrete compressive strength, carbon fixation rate and rust resistance have better performance. At the same time, by comparing Example 1 with Comparative Example 3 and Comparative Example 4, it can be seen that the carbon fixation and rust resistance effects of the mineralizer composed of mixed components are significantly better than those of the mineralizer composed of a single component.
[0102] By comparing Example 1 and Example 7, it can be seen that the amount of mineralized rust-inhibiting additive has a certain influence on the compressive strength, carbon fixation rate and rust-inhibiting performance of concrete. The more the amount of mineralized rust-inhibiting additive is added, the better the corresponding performance of the concrete is.
[0103] By comparing Example 1 and Example 2 and Comparing Example 7 and Example 9, it can be seen that the different components of the mineralizer will affect the overall rust-proof performance of the mineralized rust-proof additive. Similarly, the different components of the rust-proof additive will also affect the overall carbon fixation rate and mechanical properties of the mineralized rust-proof additive.
[0104] By comparing any one of Examples 1-12 and Comparative Examples 1-4 with the blank comparative example, it can be seen that the addition of mineralizing additives can significantly improve the compressive resistance and carbon fixation rate of concrete specimens, while enabling the concrete specimens to obtain better rust resistance, thereby solving all the technical problems reflected in the technical background of this application at one time.
[0105] Although examples of the present embodiment have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present embodiment, and the scope of the present embodiment is defined by the claims and their equivalents.
Claims
1. A mineralized rust-inhibiting additive for carbon-fixing concrete, characterized in that: The invention comprises a mineralizer, a rust inhibitor and a catalyst, wherein the mineralizer comprises at least one of calcium carbonate, calcium silicate and calcium hydroxide; The rust inhibitor includes at least one of sodium chromate, sodium molybdate and sodium zincate.
2. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 1, characterized in that: In parts by weight, the mineralizer comprises 75 to 90 parts, the rust inhibitor 7 to 20 parts, and the catalyst 3 to 5 parts.
3. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 1, characterized in that: The catalyst comprises: maleic acid, distilled water, potassium hydroxide solution and hydrogen peroxide solution.
4. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 3, characterized in that: The catalyst is composed of maleic acid, distilled water, potassium hydroxide solution and hydrogen peroxide solution in a weight ratio of 1:1:1:0.3, and the concentration of the potassium hydroxide solution is 0.15 mol / L, and the mass fraction of the hydrogen peroxide solution is 30%.
5. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 4, characterized in that: The preparation method of the catalyst is as follows: weigh sodium hydroxide powder to prepare a 0.15 mol / L solution for use, then weigh maleic acid and distilled water, mix the two, place them in a water bath heating environment and stir them, and when they are completely dissolved, add the prepared sodium hydroxide solution and potassium hydroxide solution in proportion, stir for 1 minute, stop heating, and obtain the catalyst.
6. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 1, characterized in that: The mineralizer is composed of the calcium carbonate and the calcium silicate in a weight ratio of 1:1, or is composed of the calcium carbonate and the calcium hydroxide in a weight ratio of 4:1, or is composed of the calcium silicate and the calcium hydroxide in a weight ratio of 4:
1.
7. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 1, characterized in that: The mineralizer consists of calcium carbonate, calcium silicate and calcium hydroxide, wherein the weight ratio of the calcium carbonate, calcium silicate and calcium hydroxide is 2:2:
1.
8. The mineralized rust-inhibiting additive for carbon-fixing concrete according to claim 1, characterized in that: The rust inhibitor is composed of the sodium chromate and the sodium molybdate in a weight ratio of 1:1, or is composed of the sodium chromate and the sodium octanoate in a weight ratio of 1:1, or is composed of the sodium molybdate and the sodium octanoate in a weight ratio of 1:
1.
9. A method for using the mineralized rust inhibitor according to any one of claims 1 to 8, characterized in that: include: The mineralizer and the rust inhibitor are mixed and ground according to a certain proportion, and added into the concrete paste together with the catalyst, and the concrete paste is continuously stirred during the adding process.
10. The method for using the mineralized rust inhibitor according to claim 9, characterized in that: The added mineralized rust-inhibiting additive accounts for 10-14% of the weight of the cement in the concrete paste.