Biomass carbon self-sensing cement material as well as preparation method and application thereof
By using a combination of biomass carbon, silicon powder and water reducer, a structural-sensing cement material was prepared, which solved the problems of high price and dispersion of conductive materials in the prior art, and achieved high conductivity and Cement materials with high mechanical properties, suitable for large-scale engineering applications.
Patent Information
- Application Number
- CN202410840688.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing self-perceptual cement materials are expensive and difficult to apply on a large scale. The hydrophobicity of commonly used conductive materials leads to difficulty in dispersion, which increases the difficulty of preparation and reduces the strength of cement, making it difficult to take into account both sensing functions and structural properties.
Using biomass carbon as the conductive material, amorphous carbon nanoparticles are prepared by mixing biomass with polyol solutions, solid-liquid separation, steam explosion, alkali irrigation, carbonization and alkali activation, combined with silicon powder and water reducing agent to form good Cement materials with electrical conductivity and mechanical properties.
It realizes structural-sensing integration, reduces preparation costs, improves the conductive and mechanical properties of cement materials, has good electromagnetic induction performance and high hardness, and is suitable for large-scale engineering applications.
Smart Images

Figure CN118930136A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of cement materials, and in particular relates to a biomass carbon self-sensing cement material and a preparation method and application thereof. Background Art
[0002] Cement materials have become the most consumed man-made materials in infrastructure construction due to their excellent mechanical strength, outstanding durability and low cost. They are widely used in buildings, roads, bridges, tunnels and other fields. Due to adverse conditions such as long-term load, freeze-thaw cycle damage, and salt crystallization damage, cement-based materials will age or deteriorate, which will cause major safety accidents. Major civil engineering structures such as large public buildings, bridges, dams, transmission towers and offshore platforms are expensive and important. Once an accident occurs due to damage, it will cause immeasurable safety accidents, economic losses and social impacts. In order to control the changes in material properties and structural functions and avoid major damage, in some major engineering projects, the structural health will be monitored through external or embedded sensors. However, the design service life of infrastructure is often not less than 50 years. Existing sensors cannot have the same life as the infrastructure and need to be replaced or maintained, which increases the monitoring cost and workload. Therefore, the development of self-sensing cement materials for early monitoring, evaluation and early warning of infrastructure structural health has become a research focus.
[0003] Self-sensing cement materials form a conductive network inside cement-based materials by adding conductive materials. With the changes of external load, temperature and humidity, its resistivity will change accordingly. It has the sensing characteristics of sensing stress, strain, damage, temperature and humidity. Commonly used conductive materials can be divided into three categories: carbon-based (carbon fiber, carbon nanotubes, etc.), metals and their oxides (steel fiber, ZnO, etc.) and composite fillers. Among them, carbon-based conductive materials have the best effect, but they are expensive and not suitable for large-scale engineering applications. At the same time, most of the current conductive materials (including carbon-based materials) are hydrophobic materials, which are difficult to disperse and easy to agglomerate, which increases the difficulty of preparation and reduces the strength of cement. It is difficult to take into account its structural performance while having a "sensing" function. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a biomass carbon self-sensing cement material and its preparation method and application. The biomass carbon self-sensing cement material provided by the present invention has good electrical conductivity and mechanical properties, can achieve structural-sensing integration, has good hydrophilicity, and has low preparation cost.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] The present invention provides a biomass carbon self-sensing cement material, which comprises the following components by weight: 85-95 parts of cement, 0.3-0.9 parts of biomass carbon, 0.5-1.5 parts of water reducer and 32-50 parts of water;
[0007] The method for preparing biomass carbon comprises the following steps: mixing biomass with a polyol solution, separating solid from liquid, steam-exploding the obtained solid, and alkali-leaching the obtained exploded product to obtain biomass cellulose;
[0008] Carbonizing the biomass cellulose to obtain carbonized cellulose;
[0009] The carbonized cellulose is activated with alkali to obtain the biomass carbon.
[0010] Preferably, the biomass carbon self-sensing cement material also includes 7 to 16 parts of silicon powder.
[0011] Preferably, the particle size of the silicon powder is 20-50 nm.
[0012] Preferably, the temperature of the steam explosion is ≥160° C. and the pressure is ≥5.5 MPa.
[0013] Preferably, the steam explosion is performed under the condition of applying electromagnetic waves, and the frequency of the electromagnetic waves is 180-220 GHz.
[0014] Preferably, the mass ratio of the biomass to the polyol solution is 1:15 to 23;
[0015] The polyol solution includes ethylene glycol solution and / or glycerol solution.
[0016] Preferably, the water reducer includes one or more of polycarboxylate water reducer, lignin sulfonate water reducer, naphthalene sulfonate water reducer, sodium lauryl sulfate and aminosulfonate high-efficiency water reducer.
[0017] The present invention also provides a method for preparing the biomass carbon self-sensing cement material described in the above technical solution, comprising the following steps: mixing biomass carbon, a water reducer and water to obtain a wet material; mixing the wet material with cement to obtain the biomass carbon self-sensing cement material.
[0018] Preferably, when the biomass carbon self-sensing cement material further includes silicon powder, the cement and the silicon powder are first mixed, and then the obtained mixed dry material is mixed with the wet material.
[0019] The present invention also provides the use of the biomass carbon self-sensing cement material prepared by the preparation method described in the above technical solution in self-sensing cement.
[0020] The invention provides a biomass carbon self-sensing cement material, which comprises the following components by weight: 85-95 parts of cement, 0.3-0.9 parts of biomass carbon, 0.5-1.5 parts of water reducer and 32-50 parts of water; the preparation method of the biomass carbon comprises the following steps: mixing biomass with a polyol solution, separating solid from liquid, steam-exploding the obtained solid, alkali-leaching the obtained exploded product to obtain biomass cellulose; carbonizing the biomass cellulose to obtain carbonized cellulose; alkali-activating the carbonized cellulose to obtain the biomass carbon. The biomass carbon obtained by the invention is amorphous carbon, which is composed of many fine carbon nanoparticles. There are many pores and defects between the particles. The pores and defects can uniformly introduce current into cement materials, strengthen the electrical properties of other materials, make the conductive performance of the material stronger, and have strong electromagnetic induction performance. At the same time, the biomass carbon is obtained by roughly stacking molecular fragments of a graphite layer structure in parallel and irregularly. The layers or fragments are connected by a tetrahedral bonding method of a diamond structure, have high hardness, and can improve the mechanical properties of cement materials. Pure cellulose is obtained by steam explosion, and the cellulose is carbonized to generate more oxygen-containing functional groups, such as hydroxyl groups, alcohol groups, etc. in the obtained biomass carbon. The presence of these functional groups makes the surface of the biomass carbon have certain polarity and strong affinity for water. In addition, the biomass carbon is activated and modified to further improve the hydrophilicity of the biomass carbon. The addition of a water reducer improves the fluidity of the material, improves the crack resistance and early strength of the cement material, and can make the biomass carbon uniformly dispersed in the material, further improving the mechanical properties of the cement material. The experimental results show that the biomass carbon self-sensing cement material provided by the present invention has a resistivity of ρ 0 In the range of 5.6~6.1×10 4 , the compressive strength is 44.6~47.2MPa, and it has good electrical conductivity and mechanical properties.
[0021] In addition, the present invention uses biomass carbon prepared from straw to prepare self-sensing cement materials, which can not only reduce the cost of intelligent cement-based materials, but also realize the high-value utilization of biomass materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0023] Figure 1 Schematic diagram of biomass carbon self-sensing cement;
[0024] Figure 2is the XRD pattern of biomass carbon;
[0025] Figure 3 is the SEM image of biomass carbon;
[0026] Figure 4 This is the resistivity change rate of the biomass carbon self-sensing cement prepared in Example 1. DETAILED DESCRIPTION
[0027] The invention provides a biomass carbon self-sensing cement material, which comprises the following components by weight: 85-95 parts of cement, 0.3-0.9 parts of biomass carbon, 0.5-1.5 parts of water reducing agent and 32-50 parts of water.
[0028] In the present invention, unless otherwise specified, the raw materials and equipment used are commercially available products well known in the art.
[0029] The following is an explanation of biomass carbon.
[0030] In the present invention, the method for preparing biomass carbon comprises the following steps: mixing biomass with a polyol solution, separating solid from liquid, steam-exploding the obtained solid, and alkali-leaching the obtained exploded product to obtain biomass cellulose;
[0031] Carbonizing the biomass cellulose to obtain carbonized cellulose;
[0032] The carbonized cellulose is activated with alkali to obtain the biomass carbon.
[0033] The invention mixes biomass with polyol solution, separates solid and liquid, performs steam explosion on the obtained solid, and performs alkali leaching on the obtained exploded product to obtain biomass cellulose.
[0034] In the present invention, the biomass is preferably one or more of wood, straw, grain and fruit shell, more preferably straw.
[0035] In the present invention, the polyol solution is preferably one or both of ethylene glycol solution and glycerol solution, more preferably ethylene glycol solution. The concentration of the polyol solution is preferably 30-40wt%, more preferably 34-38wt%.
[0036] In the present invention, the mass ratio of the biomass to the polyol solution is preferably 1:15 to 23, more preferably 1:18 to 21, and further preferably 1:19 to 20. The present invention mixes the biomass and the polyol solution to increase the dissolution of cellulose and improve the efficiency of biomass decomposition.
[0037] In the present invention, the biomass is preferably crushed before mixing. The present invention has no special requirements for the crushing method, and conventional crushing methods in the art can be used. The particle size of the biomass after crushing is preferably ≤3 cm, more preferably ≤1 cm.
[0038] In the present invention, the mixing temperature is preferably 100 to 120° C., more preferably 110 to 115° C., and the mixing time is preferably 0.5 to 2 h, more preferably 1 to 1.5 h.
[0039] The present invention has no special requirements for the mixing method, and conventional technical means in the art, such as stirring, can be used.
[0040] The present invention has no special requirements for the solid-liquid separation, and conventional technical means in the art may be used, such as filtration, centrifugation, etc.
[0041] Before the steam explosion, the present invention preferably first dries the obtained solid. The present invention has no special requirements for the drying, and conventional technical means in the art can be used. In a specific embodiment of the present invention, air drying is used.
[0042] In the present invention, the temperature of the steam explosion is preferably ≥160°C, more preferably 160-200°C, and further preferably 180-190°C, and the pressure is preferably ≥5.5MPa, more preferably 5.5-15MPa, and further preferably 8-12MPa. The present invention utilizes steam explosion to separate cellulose and hemicellulose in biomass. The present invention controls the temperature and pressure of steam explosion within the above range, thereby achieving material separation without wasting energy.
[0043] In the present invention, the steam explosion is preferably carried out under the condition of applying electromagnetic waves, the frequency of the electromagnetic waves is preferably 180-220 GHz, more preferably 190-210 GHz, and further preferably 200 GHz. The duration of the electromagnetic waves is preferably 20-60 min, and more preferably 30-40 min.
[0044] The present invention has no special requirements for the specific implementation of the steam explosion, and an implementation method well known in the art can be adopted. Specifically, biomass is loaded into a reactor, and high-temperature (not less than 160° C.) and high-pressure water vapor is introduced into the reactor to make the pressure in the reactor not less than 5.5 MPa. During this period, electromagnetic waves are applied to the biomass for 20 to 60 minutes, and then the air valve is opened quickly (<1s) to instantly reduce the pressure to atmospheric pressure, so that the biomass is steamed and exploded to achieve hemicellulose separation.
[0045] In the present invention, the alkaline solution used in the alkaline leaching is preferably a sodium hydroxide solution or a potassium hydroxide solution, more preferably a sodium hydroxide solution. The concentration of the alkaline solution is preferably 5-15wt%, more preferably 8-12wt%, and further preferably 10wt%. The mass ratio of the explosive product to the alkaline solution is preferably 1:2-4, more preferably 1:2.5-3.5, and further preferably 1:3.
[0046] In the present invention, the temperature of the alkali leaching is preferably 80-110° C., more preferably 90-100° C., and the time is preferably 3-8 hours, more preferably 4-6 hours. The present invention utilizes alkali leaching to remove lignin to obtain high-purity biomass cellulose.
[0047] After obtaining the biomass cellulose, the present invention carbonizes the biomass cellulose to obtain carbonized cellulose.
[0048] In the present invention, the carbonization temperature is preferably 450-600°C, more preferably 480-550°C, further preferably 500-520°C, the time is preferably 110-150min, more preferably 120-140min, further preferably 130-135min, and the carbonization heating rate is preferably 1-5°C / min, more preferably 3°C / min.
[0049] After obtaining the carbonized cellulose, the present invention performs alkali activation on the carbonized cellulose to obtain the biomass carbon.
[0050] In the present invention, the alkali activator used for the alkali activation is preferably potassium hydroxide or sodium hydroxide, more preferably sodium hydroxide, and the mass ratio of the carbonized cellulose to the alkali activator is preferably 1:1-3, more preferably 1:2. In the present invention, the alkali activation preferably includes: mixing the carbonized cellulose, the alkali activator and water, drying the obtained mixture, and calcining. The present invention has no special requirements for the amount of water used, as long as the alkali activator and the carbonized biomass cellulose are completely impregnated.
[0051] In the present invention, the drying is preferably oven drying, the oven drying temperature is preferably 90-110°C, more preferably 100°C; the calcination temperature is preferably 550-650°C, more preferably 600°C, the calcination time is preferably 1-3h, more preferably 1.5-2.5h, the calcination heating rate is preferably 1-5°C / min, more preferably 3°C / min. Calcination promotes biochar activation.
[0052] The biomass carbon self-sensing cement material is described below.
[0053] In terms of mass fraction, the biomass carbon self-sensing cement material described in the present invention includes 0.3 to 0.9 parts of biomass carbon, preferably 0.4 to 0.8 parts, and more preferably 0.5 to 0.7 parts. The biomass carbon obtained by the present invention is amorphous carbon, composed of many fine carbon nanoparticles, and there are many pores and defects between the particles. These pores and defects can evenly introduce current into the cement material, strengthen the electrical properties of other materials, and make the conductive performance of the material stronger, with strong electromagnetic induction performance. At the same time, the biomass carbon is obtained by roughly stacking molecular fragments of a graphite layer structure in parallel and irregularly, and the layers or fragments are connected by a diamond structure tetrahedral bonding method, which has a high hardness and can improve the mechanical properties of the cement material; the surface of the biomass carbon contains a large number of polar groups, such as hydroxyl groups, alcohol groups, etc., and has a strong affinity for water.
[0054] Based on the mass fraction of the biomass carbon, the biomass carbon self-sensing cement material includes 0.5 to 1.5 parts of water reducer, preferably 0.7 to 1.3 parts, and more preferably 0.9 to 1.1 parts. The water reducer preferably includes one or more of polycarboxylic acid water reducer, lignin sulfonate water reducer, naphthalene sulfonate water reducer, sodium dodecyl sulfate and aminosulfonate high-efficiency water reducer, more preferably one or more of polycarboxylic acid water reducer, lignin sulfonate water reducer and naphthalene sulfonate water reducer, and further preferably polycarboxylic acid water reducer. In the present invention, the addition of water reducer improves the fluidity of the material, improves the crack resistance and early strength of the cement material, and can make the biomass carbon evenly dispersed in the material, further improving the mechanical properties of the cement material.
[0055] Based on the mass fraction of the biomass carbon, the biomass carbon self-sensing cement material includes 85 to 95 parts of cement, preferably 88 to 93 parts, and more preferably 89 to 91 parts. The cement is preferably silicate cement, and the specification of the silicate cement is preferably 42.5, 42.5R, 52.5 or 52.5R. In the specific embodiment of the present invention, 42.5 silicate cement is used.
[0056] Based on the mass fraction of the biomass carbon, the biomass carbon self-sensing cement material includes 32 to 50 parts of water, preferably 38 to 45 parts, and more preferably 40 to 43 parts.
[0057] In the present invention, based on the mass fraction of the biomass carbon, the biomass carbon self-sensing cement material preferably also includes 7 to 16 parts of silicon powder, more preferably 9 to 13 parts, and more preferably 10 to 12 parts. The particle size of the silicon powder is preferably 20 to 50 nm, more preferably 25 to 40 nm, and further preferably 30 to 35 nm. The addition of silicon powder can further promote the dispersion of biomass carbon, cooperate with the water reducer, and improve the mechanical properties of the cement material.
[0058] The biomass carbon in the biomass carbon self-sensing cement material obtained by the present invention provides high electrical conductivity for the cement material. At the same time, there are polar groups on the surface of the biomass carbon, which can be evenly dispersed in water, thereby improving the mechanical strength of the cement material. The addition of a water reducer improves the fluidity of the material, allowing the biomass carbon to be evenly dispersed in the material, further improving the mechanical strength of the cement material.
[0059] The present invention also provides a method for preparing the biomass carbon self-sensing cement material described in the above technical solution, comprising mixing biomass carbon, a water reducer and water to obtain a wet material; and mixing the wet material with cement to obtain the biomass carbon self-sensing cement material.
[0060] The present invention has no special requirements for the mixing, and the common means in the art are used to uniformly mix the biomass carbon, water reducer and water, and uniformly mix the wet material and cement. In the specific embodiment of the present invention, mixing is performed by stirring.
[0061] In the present invention, when the biomass carbon self-sensing cement material includes silicon powder, it is preferred that the cement and the silicon powder are mixed before the wet material is mixed with the cement. The present invention has no special requirements for the mixing, and the common means in the art can be used.
[0062] The present invention also provides the use of the biomass carbon self-sensing cement material prepared by the preparation method described in the above technical solution in self-sensing cement.
[0063] In the present invention, the method for preparing the self-sensing cement preferably includes: pouring the biomass carbon self-sensing cement material into a mold, inserting a copper electrode, vibrating, standing, demolding, and curing to obtain the self-sensing cement. Figure 1 Schematic diagram of biomass carbon self-sensing cement.
[0064] In the present invention, the frequency of the vibration is preferably 45-55 Hz, and the time is preferably 20-40 seconds. Vibration is used to expel air from the biomass carbon self-sensing cement material to avoid the formation of holes after hardening, which affects the quality of cement.
[0065] In the present invention, the step of allowing the sample to stand is preferably performed by covering the sample with a cloth, and the step of allowing the sample to stand is preferably performed for 20 to 30 hours.
[0066] There is no special requirement for the demoulding in the present invention, and the demoulding can be performed by using conventional techniques in the art.
[0067] In the present invention, the curing is preferably carried out in a steam curing box, the curing temperature is preferably 85 to 95° C., and the curing time is preferably 45 to 50 hours.
[0068] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Any modification, equivalent replacement, improvement, etc. made to the implementation methods of the present invention based on the technical essence and general principles of the present invention without creative work should be within the scope of protection of the present invention.
[0069] Preparation of biomass carbon
[0070] The straw was used as the raw material, crushed, and placed in a 40wt% ethylene glycol solution at 120°C for 1h, at which time the mass ratio of the straw to the ethylene glycol solution was 1:20, solid-liquid separation, and drying to obtain the modified straw solid. The components were separated by steam explosion technology, and the modified straw dispersion was loaded into a reactor, and 160°C, 5.5MPa water vapor was introduced into the reactor to make the pressure in the reactor ≥5.5Mpa, and 200GHz electromagnetic waves were applied to the modified straw for 30min, and the air valve was opened within <1s to obtain hemicellulose. The hemicellulose was placed in a 10wt% NaOH solution until it was completely immersed, soaked at 90°C for 5h, taken out, washed with water until neutral, and dried to obtain high-purity straw cellulose.
[0071] The high-purity straw cellulose was placed in a tube furnace at 3℃ / min -1 The temperature was raised to 500°C at a rate of 1:2, kept at that temperature for 120 min, and cooled to obtain carbonized cellulose. Carbonized cellulose and KOH were mixed in water at a mass ratio of 1:2, dried at 100°C, and then heated at 3°C / min. -1 The temperature was raised to 600°C at a rate of 100 °C and kept at that temperature for 120 min to obtain biomass charcoal.
[0072] Figure 2 is the XRD pattern of biomass carbon. Figure 2 It can be seen that two broad peaks appear at around 22° and 43°, corresponding to the (002) and (100) crystal plane diffraction peaks of the graphite structure. The two diffraction peaks have large half-peak widths and low peak intensities, indicating that the biomass material has been basically carbonized and is mainly amorphous carbon.
[0073] Figure 3 This is the SEM image of biomass carbon. Figure 3 It can be seen that biomass materials have many pores and defects. These pores and defects can evenly conduct current into cement materials, strengthen the electrical properties of other materials, and make the conductive properties of materials stronger.
[0074] Example 1
[0075] Weigh 90kg 42.5 cement, 10kg 20nm silica fume, 40kg water, 0.8kg polycarboxylic acid high-performance water reducer (standard liquid polycarboxylic acid high-performance water reducer, in line with the product standard "Polycarboxylic acid high-performance water reducer" JG / T 223-2017), and 0.45kg biomass carbon. Pour the cement and silica fume into a blender and stir at 140r / min for 1min to obtain a mixed dry material. Add the polycarboxylic acid high-efficiency water reducer and biomass carbon into water and mix well to obtain a wet material. Add the wet material into the mixed dry material blender and stir at 140r / min for 30s, then stir at 200r / min for 60s to obtain a biomass carbon cement material.
[0076] Example 2
[0077] The only difference from Example 1 is that the biomass carbon is 0.9 kg, and other conditions are the same as Example 1.
[0078] Comparative Example 1
[0079] The only difference from Example 1 is that the biomass carbon is 0 kg and the lignin sulfonate is 0 kg. Other conditions are the same as those in Example 1.
[0080] Comparative Example 2
[0081] Weigh 90kg 42.5 cement, 10kg 20nm silicon powder, 40kg water, 0.8kg polycarboxylic acid high-performance water reducer, and 0.9kg carbon nanotubes. Pour the cement and silicon powder into a blender and stir at 140r / min for 1min to obtain a mixed dry material. Add the polycarboxylic acid high-efficiency water reducer and carbon nanotubes into water and ultrasonically disperse for 15min to obtain a mixed solution. Add the mixed solution into the mixed dry material blender, stir at 140r / min for 30s, and then stir at 200r / min for 60s to obtain a biomass carbon cement material.
[0082] The biomass carbon cement material obtained in Example 1 was poured into a 20×20×20mm cubic mold, and two 18×18mm copper meshes were inserted as electrodes. The copper meshes were made of copper wires with a diameter of 0.5mm. Copper wires were tied to the upper ends of the copper meshes, and the mold was pulled out, placed on an electric vibrating table and vibrated at 50Hz for 30s, covered with a material cloth, and placed at room temperature for 24 hours before demoulding. The biomass carbon self-sensing cement was cured in a 90℃ steam curing box for 48h to obtain the copper mesh installation structure reference Figure 1 .
[0083] Since the biomass conductive material is added to the cement material, a conductive network can be constructed. Without the effect of external load, the conductive materials establish a certain conductive path due to mutual contact or tunnel effect, which greatly reduces the resistivity of the cement material. When the initial load of the sensor is measured by a digital multimeter, the resistivity is recorded as ρ0 Under load, the distance between conductive materials is reduced due to deformation of cement materials, the probability of conductive materials contacting each other or tunneling increases, and the conductive path increases, resulting in a further decrease in resistivity. At this time, ρ<ρ 0 . Resistivity change rate (FCR = (ρ-ρ 0 ) / ρ 0 ) and the external load F show a certain functional change rule, that is, F = a*FCR+b. Through the relationship, the external load on the structure can be obtained, and then the structural state can be monitored and judged.
[0084] The compressive strength test refers to GB / T50081 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", and the loading rate is 0.5MPa / s.
[0085] Table 1 Test data of cement obtained from Examples 1 to 2 and Comparative Examples 1 to 2
[0086] Example 1 Example 2 Comparative Example 1 Comparative Example 2 <![CDATA[Resistivity ρ 0 (Ω·cm)]]> <![CDATA[6.1×10 4 ]]> <![CDATA[5.6×10 4 ]]> <![CDATA[10 7 ]]> <![CDATA[5.5×10 4 ]]> Compressive strength MPa 47.2 44.6 45 40.8
[0087] It can be seen from Table 1 that the resistivity of the cement material obtained in Examples 1-2 is comparable to that of the cement material obtained using carbon nanotubes in Comparative Example 2. However, the compressive strength of the cement material obtained in Examples 1-2 is higher than that of the cement material obtained using carbon nanotubes, indicating that the biochar obtained in the present invention can reduce the resistivity of cement and ensure the strength of cement.
[0088] Figure 4 The resistivity change rate of the biomass carbon self-sensing cement prepared in Example 1. The cement obtained from the biomass carbon cement material was subjected to a cyclic load with a peak load of 5 MPa at a rate of 0.2 MPa / s. The resistivity change rate of the biomass carbon cement material changed regularly with the load change. Figure 4 It can be seen that the biomass carbon cement prepared in the present invention has the sensing property of sensing stress.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A biomass carbon self-sensing cement material, characterized in that: The composition comprises the following components by weight: 85-95 parts of cement, 0.3-0.9 parts of biomass carbon, 0.5-1.5 parts of water reducing agent and 32-50 parts of water; The method for preparing biomass carbon comprises the following steps: mixing biomass with a polyol solution, separating solid from liquid, steam-exploding the obtained solid, and alkali-leaching the obtained exploded product to obtain biomass cellulose; Carbonizing the biomass cellulose to obtain carbonized cellulose; The carbonized cellulose is activated with alkali to obtain the biomass carbon.
2. The biomass carbon self-sensing cement material according to claim 1, characterized in that: The biomass carbon self-sensing cement material also includes 7 to 16 parts of silicon powder.
3. The biomass carbon self-sensing cement material according to claim 2, characterized in that: The particle size of the silicon powder is 20 to 50 nm.
4. The biomass carbon self-sensing cement material according to claim 1, characterized in that: The temperature of the steam explosion is ≥160°C, and the pressure is ≥5.5MPa.
5. The biomass carbon self-sensing cement material according to claim 1 or 4, characterized in that: The steam explosion is performed under the condition of applying electromagnetic waves, and the frequency of the electromagnetic waves is 180-220 GHz.
6. The biomass carbon self-sensing cement material according to claim 1, characterized in that: The mass ratio of the biomass to the polyol solution is 1:15-23; The polyol solution includes ethylene glycol solution and / or glycerol solution.
7. The biomass carbon self-sensing cement material according to claim 1, characterized in that: The water reducer includes one or more of polycarboxylate water reducer, lignin sulfonate water reducer, naphthalene sulfonate water reducer, sodium lauryl sulfate and aminosulfonate high-efficiency water reducer.
8. The method for preparing the biomass carbon self-sensing cement material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing biomass carbon, a water reducing agent and water to obtain a wet material; The wet material is mixed with cement to obtain the biomass carbon self-sensing cement material.
9. The preparation method according to claim 8, characterized in that: When the biomass carbon self-sensing cement material also includes silicon powder, the cement and the silicon powder are first mixed, and then the obtained mixed dry material is mixed with the wet material.
10. Use of the biomass carbon self-sensing cement material according to any one of claims 1 to 7 or the biomass carbon self-sensing cement material prepared by the preparation method according to any one of claims 8 to 9 in self-sensing cement.
Citation Information
Patent Citations
Preparation method of biochar with good electrical property
CN108658056A
Self-induction conductive cement composite material and preparation method thereof
CN115385621A
Battery module
KR1020250137799A
Cementitious biochar compositions and methods of making the same
US20220298073A1
Cited By
Method for preparing highly-lignified biomass-based hard carbon material through water / alcohol synergistic auxiliary steam explosion, hard carbon material and sodium ion battery
CN119143114A