Preparation method of ultra-high performance cement-based material doped with waste glass powder

By incorporating waste glass powder into the preparation method of ultra-high performance cement-based materials, and utilizing magnetorheological fluid technology, microencapsulated phase change materials, and carbon dioxide curing technology, the problems of density, durability, and environmental protection of traditional cement-based materials have been solved, and the high performance and environmental protection of the materials have been improved.

CN118930146AActive Publication Date: 2024-11-12FUJIAN HUIFENG CONSTR TECH CO LTD

Patent Information

Application Number
CN202411059714.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Traditional cement-based materials have shortcomings in terms of density, durability, environmental friendliness, and workability. They are particularly susceptible to freeze-thaw cycles in cold regions, leading to cracking and poor durability.

Method used

An ultra-high performance cement-based material preparation method incorporating waste glass powder is adopted. The material is compacted using magnetorheological fluid technology, combined with microencapsulated phase change materials and carbon dioxide curing technology to regulate the internal temperature of the material, improve its density and durability, and use a green and efficient water-reducing agent to improve its construction performance.

Benefits of technology

It significantly improves the density and durability of materials, reduces energy consumption and pollution, enhances freeze-thaw resistance and impermeability, and meets the high requirements of engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930146A_ABST
    Figure CN118930146A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building material preparation, and discloses a preparation method of an ultra-high performance cement-based material doped with waste glass powder, and the preparation method comprises the following steps: S1, providing cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, a phase change material, a green high-efficiency water reducing agent and steel fiber; s2, dispersing graphene in deionized water to form a graphene suspension; s3, carrying out microencapsulation treatment on the phase change material; s4, cement, waste glass powder, silica fume, fine aggregate and nano titanium dioxide are subjected to dry mixing, and a basic mixture is formed. The compactness and durability of the material are remarkably improved by adopting a magnetorheological fluid technology for compaction, microencapsulation of the phase change material and a carbon dioxide curing technology, and meanwhile, by adjusting the temperature and forming a carbonization layer, the freeze-thaw resistance and the permeation resistance are improved, and the service life is prolonged. In addition, environment-friendly materials and a high-efficiency water reducing agent are adopted, so that the preparation process is more energy-saving and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material preparation, in particular to a method for preparing an ultra-high performance cement-based material mixed with waste glass powder. Background Art

[0002] With the rapid development of the global construction industry and the acceleration of urbanization, cement-based materials are increasingly used in construction projects. Cement-based materials have become the main choice of building materials due to their low cost, strong plasticity and wide range of applications. However, with the advancement of technology and the improvement of construction standards, the performance of traditional cement-based materials can no longer fully meet the requirements of modern buildings for high strength, high durability and environmental protection.

[0003] In the production process of traditional cement-based materials, cement, as the main cementitious material, reacts with aggregate and water to form a solid material with certain strength and durability. In order to improve the performance of cement-based materials, researchers have been trying various methods, such as adding mineral admixtures (such as silica fume, fly ash and slag) to improve the strength and durability of the material. Silica fume is widely used as an important admixture to improve the performance of cement-based materials due to its ultrafine particles and high activity.

[0004] In recent years, waste glass powder (WGP) has been gradually introduced into cement-based materials as a mineral admixture. Studies have found that the addition of waste glass powder can not only effectively reduce the amount of cement used and reduce carbon dioxide emissions, but also significantly improve the performance of cement-based materials.

[0005] Although these methods have achieved some results to a certain extent, they still face many challenges. For example, traditional mechanical vibration compaction methods are prone to produce bubbles and voids, resulting in insufficient density and strength of the material. In addition, cement-based materials will be affected by environmental factors such as temperature changes, humidity changes, and chemical erosion during long-term use, causing microcracks to form inside the material and gradually expand, affecting its durability. In cold areas, freeze-thaw cycles are an important factor affecting the durability of cement-based materials. Traditional materials are prone to cracking and peeling after multiple freeze-thaw cycles. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing an ultra-high performance cement-based material mixed with waste glass powder, which solves the problems of cement-based materials mixed with non-glass powder in terms of density, durability, environmental protection and construction performance.

[0007] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing an ultra-high performance cement-based material mixed with waste glass powder, comprising the following steps:

[0008] S1. Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, phase change material, green high-efficiency water reducing agent and steel fiber;

[0009] S2, dispersing graphene in deionized water to form a graphene suspension;

[0010] S3, microencapsulating the phase change material;

[0011] S4, dry-mixing cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide to form a basic mixture;

[0012] S5, wet mixing the base mixture, the graphene suspension, and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed;

[0013] S6. Gradually add green high-efficiency water reducer during wet mixing to adjust the working performance of the mixture;

[0014] S7, finally add steel fiber and continue stirring until the steel fiber is evenly distributed;

[0015] S8, pouring the mixture into a mold and compacting it using magnetorheological fluid technology;

[0016] S9. After initial setting, demoulding is performed and the sample is placed in a curing box for standard curing;

[0017] S10, during the curing period, the phase change material is heated periodically to release energy and adjust the internal temperature of the material;

[0018] S11. After curing for 28 days, the sample is subjected to high-temperature sintering treatment.

[0019] Preferably, in step S1, by weight percentage, cement is 50-70%, waste glass powder is 10-20%, silica fume is 5-15%, fine aggregate is 10-20%, nano titanium dioxide is 1-5%, graphene is 0.1-1%, phase change material is 1-5%, green high-efficiency water reducing agent is 0.5-2%, and steel fiber is 0.5-2%.

[0020] Preferably, the phase change material is selected from paraffin, fatty acid or hydrated salt, and the green high-efficiency water reducer is selected from plant-based water reducer, tannic acid or guar gum.

[0021] Preferably, the specific steps of microencapsulation treatment in step S3 include the following:

[0022] S3.1, prepare phase change material solution:

[0023] The solid phase change material is heated to a molten state, and then dissolved in an appropriate amount of water or an organic solvent to form a uniform solution;

[0024] S3.2. Prepare wall material solution:

[0025] Take gelatin and gum arabic, dissolve them in warm water at a temperature of 40-50°C, stir evenly, and form a gelatin-gum arabic composite wall material solution;

[0026] S3.3, mixing phase change material and wall material solution: slowly drip the phase change material solution into the wall material solution, stirring while adding, maintaining the temperature at 40-50°C, and the stirring rate at 300-500rpm;

[0027] S3.4, forming microcapsules: lowering the temperature of the mixed solution to 10-15°C, stirring continuously, allowing the phase change material to gradually solidify to form microcapsules, and adjusting the pH value to 4.0-4.5 to promote coprecipitation and coating of microcapsule wall materials;

[0028] S3.5. Solidification and collection: solidify the formed microcapsules by freeze drying or spray drying, collect the dried microcapsules, and sieve them to obtain microcapsule phase change materials with uniform particle size.

[0029] Preferably, the method for adjusting the working performance of the mixture in step S6 is to test the fluidity and stability of the mixture by slump test, spread test and segregation test respectively, and adjust the amount of water reducer according to the test results. The method for adjusting the amount of water reducer is:

[0030] If the fluidity is insufficient, increase the amount of water reducing agent;

[0031] If the mixture segregates, reduce the amount of water reducer or increase the proportion of fine aggregate.

[0032] Preferably, the periodic heating rule in step S10 is:

[0033] Initial settings:

[0034] Set the initial heating time to 1.5-2h, gradually raise the material temperature to the phase change temperature of the phase change material, and control the initial heating temperature to a high value within the phase change temperature range;

[0035] Heating cycle setting: The heating cycle is set to 7.5-8h once, with each heating time of 0.5-1h. In each heating cycle, the temperature is kept within the phase change temperature range;

[0036] Cooling cycle setting: After each heating, turn off the heating device and perform natural cooling for 6-7 hours. During the cooling cycle, monitor the temperature change, and the internal temperature of the material gradually drops but does not fall below room temperature;

[0037] Monitoring and adjustment: Use temperature sensors to monitor the temperature inside and on the surface of the material in real time, record temperature data, analyze the temperature changes in each heating and cooling cycle, and adjust the heating time, power and cycle based on the data analysis results to keep the temperature within the phase change temperature range.

[0038] Preferably, the initial heating temperature is controlled within the phase change temperature range with an accuracy of ±2°C.

[0039] Preferably, the curing in step S10 specifically includes the following steps:

[0040] Wet curing stage (first 7 days):

[0041] Place the demoulded samples in a wet curing box;

[0042] The temperature range of the wet curing box is set at 18-22°C, and the humidity is maintained at 90-100%;

[0043] Wet curing was continued for 7 days, and the sample surface remained moist;

[0044] Carbon dioxide curing stage (Day 8 to Day 28):

[0045] Move the wet-cured samples into a carbon dioxide curing box;

[0046] Set the temperature range of the curing box to 18-22°C and the carbon dioxide concentration to 10-20%;

[0047] Carbon dioxide curing was performed for 6-10 hours every day, and the samples were kept at room temperature for the rest of the time.

[0048] Preferably, the magnetorheological fluid technology compaction in step S8 specifically includes the following steps:

[0049] Prepare the mold and mixture: Pour the mixture into a mold pre-coated with a layer of magnetorheological fluid;

[0050] Install the electromagnetic coil: install the electromagnetic coil on the outer wall and bottom of the mold;

[0051] Set the magnetic field parameters: initial magnetic field strength 0.1-0.5T, maximum magnetic field strength 0.5-1T, magnetic field application time 3-10min;

[0052] Start magnetic field compaction: Apply different magnetic field strengths in three stages, from small to large, and monitor the compaction effect of the magnetic field and the mixture in real time through the control system to adjust the magnetic field strength and action time;

[0053] Compaction completion and curing:

[0054] After the magnetic field ends, the electromagnetic coil is turned off and the mold is left to stand for preliminary curing.

[0055] Preferably, the phase change temperature ranges of the phase change materials paraffin, fatty acid or hydrated salt are 20-60°C for paraffin, 30-70°C for fatty acid and 30-50°C for hydrated salt, respectively.

[0056] The present invention provides a method for preparing an ultra-high performance cement-based material mixed with waste glass powder. The method has the following beneficial effects:

[0057] 1. The present invention significantly improves the density of the material by using magnetorheological fluid technology for compaction, so that the rheological properties of the mixture are effectively regulated under the action of the magnetic field, bubbles are eliminated, and the microstructure is denser. Traditional mechanical vibration cannot achieve the same effect and is prone to produce bubbles and gaps, which affects the density and strength of the material.

[0058] 2. The present invention significantly improves the durability of the material through the application of microencapsulated phase change material and carbon dioxide curing technology. The microencapsulated phase change material can absorb and release energy when the temperature changes, adjust the internal temperature of the material, and reduce the damage to the material caused by temperature stress. The carbon dioxide curing technology promotes the formation of a carbonized layer on the surface of the material, improves the material's anti-freeze and anti-penetration properties, and thus extends the material's service life.

[0059] 3. The present invention adopts environmentally friendly materials such as microencapsulated phase change materials and green high-efficiency water reducing agents, making the entire preparation process more energy-saving and environmentally friendly. Compared with traditional methods, it has significant advantages in reducing energy consumption and pollution, and helps to achieve the goals of green buildings and sustainable development.

[0060] 4. The present invention promotes the formation of a carbonized layer on the surface of the material through the application of carbon dioxide curing technology, improves the material's anti-freeze-thaw and anti-permeability properties, significantly improves the material's durability, and solves the problem that traditional materials are easily damaged and have poor durability under freeze-thaw cycles and immersion in water. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0062] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0063] Example:

[0064] Please see attached Figure 1The embodiment of the present invention provides a method for preparing an ultra-high performance cement-based material mixed with waste glass powder, comprising the following steps:

[0065] S1. Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, phase change material, green high-efficiency water reducing agent and steel fiber;

[0066] S2, dispersing graphene in deionized water to form a graphene suspension;

[0067] S3, microencapsulating the phase change material;

[0068] S4, dry-mixing cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide to form a basic mixture;

[0069] S5, wet mixing the base mixture, the graphene suspension, and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed;

[0070] S6. Gradually add green high-efficiency water reducer during wet mixing to adjust the working performance of the mixture;

[0071] S7, finally add steel fiber and continue stirring until the steel fiber is evenly distributed;

[0072] S8, pouring the mixture into a mold and compacting it using magnetorheological fluid technology;

[0073] S9. After initial setting, demoulding is performed and the sample is placed in a curing box for standard curing;

[0074] S10, during the curing period, the phase change material is heated periodically to release energy and adjust the internal temperature of the material;

[0075] S11. After curing for 28 days, the sample is subjected to high-temperature sintering treatment.

[0076] In step S1, by weight percentage, cement is 50-70%, waste glass powder is 10-20%, silica fume is 5-15%, fine aggregate is 10-20%, nano titanium dioxide is 1-5%, graphene is 0.1-1%, phase change material is 1-5%, green high-efficiency water reducing agent is 0.5-2%, and steel fiber is 0.5-2%.

[0077] The phase change material can be selected from paraffin, fatty acid or hydrated salt, and the green high-efficiency water reducer can be selected from plant-based water reducer, tannic acid or guar gum.

[0078] The specific steps of microencapsulation treatment in step S3 include the following:

[0079] S3.1, prepare phase change material solution:

[0080] The solid phase change material is heated to a molten state, and then dissolved in an appropriate amount of water or an organic solvent to form a uniform solution;

[0081] S3.2. Prepare wall material solution:

[0082] Take gelatin and gum arabic, dissolve them in warm water at a temperature of 40-50°C, stir evenly, and form a gelatin-gum arabic composite wall material solution;

[0083] S3.3, mixing phase change material and wall material solution: slowly drip the phase change material solution into the wall material solution, stirring while adding, maintaining the temperature at 40-50°C, and the stirring rate at 300-500rpm;

[0084] S3.4, forming microcapsules: lowering the temperature of the mixed solution to 10-15°C, stirring continuously, allowing the phase change material to gradually solidify to form microcapsules, and adjusting the pH value to 4.0-4.5 to promote coprecipitation and coating of microcapsule wall materials;

[0085] S3.5. Solidification and collection: solidify the formed microcapsules by freeze drying or spray drying, collect the dried microcapsules, and sieve them to obtain microcapsule phase change materials with uniform particle size.

[0086] The method for adjusting the working performance of the mixture in step S6 is to test the fluidity and stability of the mixture by slump test, expansion test and segregation test respectively, and adjust the amount of water reducing agent according to the test results. The method for adjusting the amount of water reducing agent is:

[0087] If the fluidity is insufficient, increase the amount of water reducing agent;

[0088] If the mixture segregates, reduce the amount of water reducer or increase the proportion of fine aggregate.

[0089] The periodic heating rule in step S10 is:

[0090] Initial settings:

[0091] Set the initial heating time to 1.5-2h, gradually raise the material temperature to the phase change temperature of the phase change material, and control the initial heating temperature to a high value within the phase change temperature range;

[0092] Heating cycle setting: The heating cycle is set to 7.5-8h once, with each heating time of 0.5-1h. In each heating cycle, the temperature is kept within the phase change temperature range;

[0093] Cooling cycle setting: After each heating, turn off the heating device and perform natural cooling for 6-7 hours. During the cooling cycle, monitor the temperature change, and the internal temperature of the material gradually drops but does not fall below room temperature;

[0094] Monitoring and adjustment: Use temperature sensors to monitor the temperature inside and on the surface of the material in real time, record temperature data, analyze the temperature changes in each heating and cooling cycle, and adjust the heating time, power and cycle based on the data analysis results to keep the temperature within the phase change temperature range.

[0095] The initial heating temperature is controlled within the phase change temperature range with an accuracy of ±2°C.

[0096] The maintenance in step S10 specifically includes the following steps:

[0097] Wet curing stage (first 7 days):

[0098] Place the demoulded samples in a wet curing box;

[0099] The temperature range of the wet curing box is set at 18-22°C, and the humidity is maintained at 90-100%;

[0100] Wet curing was continued for 7 days, and the sample surface remained moist;

[0101] Carbon dioxide curing stage (Day 8 to Day 28):

[0102] Move the wet-cured samples into a carbon dioxide curing box;

[0103] Set the temperature range of the curing box to 18-22°C and the carbon dioxide concentration to 10-20%;

[0104] Carbon dioxide curing was performed for 6-10 hours every day, and the samples were kept at room temperature for the rest of the time.

[0105] The magnetorheological fluid technology compaction in step S8 specifically includes the following steps:

[0106] Prepare the mold and mixture: Pour the mixture into a mold pre-coated with a layer of magnetorheological fluid;

[0107] Install the electromagnetic coil: install the electromagnetic coil on the outer wall and bottom of the mold;

[0108] Set the magnetic field parameters: initial magnetic field strength 0.1-0.5T, maximum magnetic field strength 0.5-1T, magnetic field application time 3-10min;

[0109] Start magnetic field compaction: Apply different magnetic field strengths in three stages, from small to large, and monitor the compaction effect of the magnetic field and the mixture in real time through the control system to adjust the magnetic field strength and action time;

[0110] Compaction completion and curing:

[0111] After the magnetic field ends, the electromagnetic coil is turned off and the mold is left to stand for preliminary curing.

[0112] The phase change temperature ranges of the phase change materials paraffin, fatty acid or hydrated salt are 20-60°C for paraffin, 30-70°C for fatty acid and 30-50°C for hydrated salt respectively.

[0113] Embodiment 1:

[0114] Material ratio (by weight percentage):

[0115] Cement: 60%

[0116] Waste glass powder: 15%

[0117] Silica fume: 10%

[0118] Fine aggregate: 10%

[0119] Nano titanium dioxide: 2%

[0120] Graphene: 0.5%

[0121] Phase change material (paraffin): 1.5%

[0122] Green high-efficiency water reducing agent (tannic acid): 0.7%

[0123] Steel fiber: 0.3%

[0124] Implementation steps:

[0125] Materials to be provided:

[0126] Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, paraffin, tannic acid and steel fiber.

[0127] Preparation of graphene suspension:

[0128] 0.5% graphene was dispersed in deionized water to form a graphene suspension.

[0129] Microencapsulation of phase change materials:

[0130] Heat the paraffin wax to a molten state, and then dissolve it in an appropriate amount of organic solvent to form a uniform solution.

[0131] Dissolve gelatin and gum arabic in warm water at 45°C respectively, stir evenly to form a composite wall material solution.

[0132] Slowly drip the paraffin solution into the wall material solution while stirring, maintaining the temperature at 45°C and the stirring rate at 400 rpm.

[0133] The temperature of the mixed solution was lowered to 12°C, stirring was continued, and the pH value was adjusted to 4.2 to form microcapsules.

[0134] Solidification is performed by freeze drying, and the dried microcapsule paraffin is collected and sieved to obtain a microcapsule phase change material with uniform particle size.

[0135] Dry mix base mixture:

[0136] Cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide are dry-mixed to form a basic mixture.

[0137] Wet mix base mixture:

[0138] The base mixture is wet-mixed with the graphene suspension and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed.

[0139] Add green high-efficiency water reducing agent:

[0140] During the wet mixing process, tannic acid is gradually added to adjust the working properties of the mixture and ensure that the mixture has good fluidity and stability.

[0141] Adding steel fibers:

[0142] Add the steel fibers last and continue stirring until the steel fibers are evenly distributed.

[0143] Compaction with magnetorheological fluid technology:

[0144] The mixture is poured into a mold that has been pre-coated with a layer of magnetorheological fluid.

[0145] The electromagnetic coil was installed, with an initial magnetic field strength of 0.3 T, a maximum magnetic field strength of 0.7 T, and a magnetic field application time of 8 minutes.

[0146] Different magnetic field intensities were applied in three stages, and the compaction effects of the magnetic field and the mixture were monitored in real time.

[0147] Demolding and wet curing after initial setting:

[0148] Demoulding is carried out after initial setting (within 24 hours).

[0149] The demoulded samples were placed in a wet curing box with the temperature set at 20°C and the humidity maintained at 95% for 7 days.

[0150] Carbon dioxide maintenance:

[0151] The samples after wet curing were moved into a carbon dioxide curing box, the temperature was set at 20°C, the carbon dioxide concentration was controlled at 15%, carbon dioxide curing was performed for 8 hours a day, and the rest of the time was kept in room temperature.

[0152] Cyclic heating:

[0153] Initial setting: The initial heating time is 2 hours, and the material temperature is gradually raised to the phase change temperature of the phase change material (55°C).

[0154] The heating cycle was set to once every 8 hours, with each heating lasting 1 hour, and the temperature was kept within the phase change temperature range.

[0155] Cooling cycle setting: After each heating, natural cooling is carried out for 7 hours, and the temperature changes are monitored. The temperature is not lower than room temperature.

[0156] High temperature sintering treatment:

[0157] After curing for 28 days, the samples were sintered at high temperature with the temperature set at 900°C for 3 hours.

[0158] Summary of Example 1:

[0159] Through the above steps, an ultra-high performance cement-based material mixed with waste glass powder was prepared, compacted using magnetorheological fluid technology, and combined with wet curing and carbon dioxide curing to improve the density and durability of the material.

[0160] Embodiment 2:

[0161] Material ratio (by weight percentage):

[0162] Cement: 65%

[0163] Waste glass powder: 12%

[0164] Silica fume: 10%

[0165] Fine aggregate: 8%

[0166] Nano titanium dioxide: 2%

[0167] Graphene: 1%

[0168] Phase change material (fatty acid): 1.5%

[0169] Green high-efficiency water reducing agent (guar gum): 0.5%

[0170] Steel fiber: 0.5%

[0171] Implementation steps:

[0172] Materials to be provided:

[0173] Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, fatty acid, guar gum and steel fiber.

[0174] Preparation of graphene suspension:

[0175] 1% graphene was dispersed in deionized water to form a graphene suspension.

[0176] Microencapsulation of phase change materials:

[0177] The fatty acid is heated to a molten state and then dissolved in an appropriate amount of an organic solvent to form a uniform solution.

[0178] Dissolve gelatin and gum arabic in warm water at 45°C respectively, stir evenly to form a composite wall material solution.

[0179] Slowly drip the fatty acid solution into the wall material solution while stirring, maintaining the temperature at 45°C and the stirring rate at 400 rpm.

[0180] The temperature of the mixed solution was lowered to 12°C, stirring was continued, and the pH value was adjusted to 4.2 to form microcapsules.

[0181] Solidification is performed by freeze drying, and the dried microcapsule fatty acid is collected and sieved to obtain a microcapsule phase change material with uniform particle size.

[0182] Dry mix base mixture:

[0183] Cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide are dry-mixed to form a basic mixture.

[0184] Wet mix base mixture:

[0185] The base mixture is wet-mixed with the graphene suspension and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed.

[0186] Add green high-efficiency water reducing agent:

[0187] During the wet mixing process, guar gum is gradually added to adjust the working properties of the mixture to ensure that the mixture has good fluidity and stability.

[0188] Adding steel fibers:

[0189] Add the steel fibers last and continue stirring until the steel fibers are evenly distributed.

[0190] Compaction with magnetorheological fluid technology:

[0191] The mixture is poured into a mold that has been pre-coated with a layer of magnetorheological fluid.

[0192] The electromagnetic coil was installed, with an initial magnetic field strength of 0.4 T, a maximum magnetic field strength of 0.8 T, and a magnetic field application time of 9 minutes.

[0193] Different magnetic field intensities were applied in three stages, and the compaction effects of the magnetic field and the mixture were monitored in real time.

[0194] Demolding and wet curing after initial setting:

[0195] Demoulding is carried out after initial setting (within 24 hours).

[0196] The demoulded samples were placed in a wet curing box with the temperature set at 20°C and the humidity maintained at 95% for 7 days.

[0197] Carbon dioxide maintenance:

[0198] The samples after wet curing were moved into a carbon dioxide curing box, the temperature was set at 20°C, the carbon dioxide concentration was controlled at 15%, carbon dioxide curing was performed for 8 hours a day, and the rest of the time was kept in room temperature.

[0199] Cyclic heating:

[0200] Initial setting: The initial heating time is 1.5 hours, and the material temperature is gradually raised to the phase change temperature of the phase change material (50°C).

[0201] The heating cycle was set to once every 7.5 hours, with each heating time of 0.5 hours, and the temperature was maintained within the phase transition temperature range.

[0202] Cooling cycle setting: After each heating, perform natural cooling for 6.5 hours, monitor temperature changes, and the temperature should not be lower than room temperature.

[0203] High temperature sintering treatment:

[0204] After curing for 28 days, the samples were sintered at high temperature with the temperature set at 850°C for 3 hours.

[0205] Summary of Example 2:

[0206] Through the above steps, on the basis of Example 1, the material ratio and the type of phase change material were adjusted, guar gum was used as a green and efficient water reducer, the parameters of the magnetorheological fluid technology compaction and the time setting of the periodic heating were optimized, and the performance of the material was further improved.

[0207] Embodiment three:

[0208] Material ratio (by weight percentage):

[0209] Cement: 62%

[0210] Waste glass powder: 14%

[0211] Silica fume: 10%

[0212] Fine aggregate: 9%

[0213] Nano titanium dioxide: 2%

[0214] Graphene: 0.8%

[0215] Phase change material (hydrated salt): 1.5%

[0216] Green high-efficiency water reducer (plant-based water reducer): 0.7%

[0217] Steel fiber: 0.3%

[0218] Implementation steps:

[0219] Materials to be provided:

[0220] Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, hydrated salt, plant-based water reducer and steel fiber.

[0221] Preparation of graphene suspension:

[0222] 0.8% graphene was dispersed in deionized water to form a graphene suspension.

[0223] Microencapsulation of phase change materials:

[0224] The hydrated salt is heated to a molten state and then dissolved in an appropriate amount of an organic solvent to form a uniform solution.

[0225] Dissolve gelatin and gum arabic in warm water at 45°C respectively, stir evenly to form a composite wall material solution.

[0226] Slowly drip the hydrated salt solution into the wall material solution while stirring, maintaining the temperature at 45°C and the stirring rate at 400 rpm.

[0227] The temperature of the mixed solution was lowered to 12°C, stirring was continued, and the pH value was adjusted to 4.2 to form microcapsules.

[0228] Solidification is performed by freeze drying, and the dried microcapsule hydrated salt is collected and sieved to obtain a microcapsule phase change material with uniform particle size.

[0229] Dry mix base mixture:

[0230] Cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide are dry-mixed to form a basic mixture.

[0231] Wet mix base mixture:

[0232] The base mixture is wet-mixed with the graphene suspension and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed.

[0233] Add green high-efficiency water reducing agent:

[0234] During the wet mixing process, plant-based water reducer is gradually added to adjust the working properties of the mixture and ensure that the mixture has good fluidity and stability.

[0235] Adding steel fibers:

[0236] Add the steel fibers last and continue stirring until the steel fibers are evenly distributed.

[0237] Compaction with magnetorheological fluid technology:

[0238] The mixture is poured into a mold that has been pre-coated with a layer of magnetorheological fluid.

[0239] The electromagnetic coil was installed, with an initial magnetic field strength of 0.4 T, a maximum magnetic field strength of 0.9 T, and a magnetic field application time of 10 minutes.

[0240] Different magnetic field intensities were applied in three stages, and the compaction effects of the magnetic field and the mixture were monitored in real time.

[0241] Demolding and wet curing after initial setting:

[0242] Demoulding is carried out after initial setting (within 24 hours).

[0243] The demoulded samples were placed in a wet curing box with the temperature set at 20°C and the humidity maintained at 95% for 7 days.

[0244] Carbon dioxide maintenance:

[0245] The samples after wet curing were moved into a carbon dioxide curing box, the temperature was set at 20°C, the carbon dioxide concentration was controlled at 15%, carbon dioxide curing was performed for 8 hours a day, and the rest of the time was kept in room temperature.

[0246] Cyclic heating:

[0247] Initial setting: The initial heating time is 1.5 hours, and the material temperature is gradually raised to the phase change temperature of the phase change material (45°C).

[0248] The heating cycle was set to once every 8 hours, with each heating lasting 1 hour, and the temperature was kept within the phase change temperature range.

[0249] Cooling cycle setting: After each heating, natural cooling is carried out for 7 hours, and the temperature changes are monitored. The temperature is not lower than room temperature.

[0250] High temperature sintering treatment:

[0251] After curing for 28 days, the samples were sintered at high temperature with the temperature set at 900°C for 3 hours.

[0252] Summary of Example 3:

[0253] On the basis of Example 2, the material ratio and the type of phase change material were adjusted, a plant-based water reducer was used, and the parameters of the magnetorheological fluid technology compaction and the temperature setting of the periodic heating were further optimized to improve the overall performance of the material.

[0254] Embodiment 4:

[0255] Material ratio (by weight percentage):

[0256] Cement: 64%

[0257] Waste glass powder: 12%

[0258] Silica fume: 10%

[0259] Fine aggregate: 9%

[0260] Nano titanium dioxide: 2%

[0261] Graphene: 0.6%

[0262] Phase change material (paraffin): 1.5%

[0263] Green high-efficiency water reducing agent (tannic acid): 0.7%

[0264] Steel fiber: 0.5%

[0265] Implementation steps:

[0266] Materials to be provided:

[0267] Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, paraffin, tannic acid and steel fiber.

[0268] Preparation of graphene suspension:

[0269] 0.6% graphene was dispersed in deionized water to form a graphene suspension.

[0270] Microencapsulation of phase change materials:

[0271] Heat the paraffin wax to a molten state, and then dissolve it in an appropriate amount of organic solvent to form a uniform solution.

[0272] Dissolve gelatin and gum arabic in warm water at 45°C respectively, stir evenly to form a composite wall material solution.

[0273] Slowly drip the paraffin solution into the wall material solution while stirring, maintaining the temperature at 45°C and the stirring rate at 400 rpm.

[0274] The temperature of the mixed solution was lowered to 12°C, stirring was continued, and the pH value was adjusted to 4.2 to form microcapsules.

[0275] The microcapsule paraffin is collected and solidified by freeze drying, and the microcapsule phase change material with uniform particle size is obtained by sieving.

[0276] Dry mix base mixture:

[0277] Cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide are dry-mixed to form a basic mixture.

[0278] Wet mix base mixture:

[0279] The base mixture is wet-mixed with the graphene suspension and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed.

[0280] Add green high-efficiency water reducing agent:

[0281] During the wet mixing process, tannic acid is gradually added to adjust the working properties of the mixture and ensure that the mixture has good fluidity and stability.

[0282] Adding steel fibers:

[0283] Add the steel fibers last and continue stirring until the steel fibers are evenly distributed.

[0284] Compaction with magnetorheological fluid technology:

[0285] The mixture is poured into a mold that has been pre-coated with a layer of magnetorheological fluid.

[0286] The electromagnetic coil was installed with an initial magnetic field strength of 0.3 T, a maximum magnetic field strength of 1 T, and a magnetic field application time of 10 minutes.

[0287] Different magnetic field intensities were applied in three stages, and the compaction effects of the magnetic field and the mixture were monitored in real time.

[0288] Demolding and wet curing after initial setting:

[0289] Demoulding is carried out after initial setting (within 24 hours).

[0290] The demoulded samples were placed in a wet curing box with the temperature set at 20°C and the humidity maintained at 95% for 7 days.

[0291] Carbon dioxide maintenance:

[0292] The samples after wet curing were moved into a carbon dioxide curing box, the temperature was set at 20°C, the carbon dioxide concentration was controlled at 15%, carbon dioxide curing was performed for 8 hours a day, and the rest of the time was kept in room temperature.

[0293] Cyclic heating:

[0294] Initial setting: The initial heating time is 2 hours, and the material temperature is gradually raised to the phase change temperature of the phase change material (55°C).

[0295] The heating cycle was set to once every 8 hours, with each heating lasting 1 hour, and the temperature was kept within the phase change temperature range.

[0296] Cooling cycle setting: After each heating, natural cooling is carried out for 7 hours, and the temperature changes are monitored. The temperature is not lower than room temperature.

[0297] High temperature sintering treatment:

[0298] After curing for 28 days, the samples were sintered at high temperature with the temperature set at 900°C for 3 hours.

[0299] Summary of Example 4:

[0300] On the basis of Example 3, the material ratio was optimized, the parameters of magnetorheological fluid technology compaction were improved, and the temperature and time settings of periodic heating were further adjusted, which significantly improved the overall performance and durability of the material.

[0301] Embodiment five:

[0302] Material ratio (by weight percentage):

[0303] Cement: 63%

[0304] Waste glass powder: 14%

[0305] Silica fume: 9%

[0306] Fine aggregate: 9%

[0307] Nano titanium dioxide: 2%

[0308] Graphene: 0.8%

[0309] Phase change material (fatty acid): 1.5%

[0310] Green high-efficiency water reducer (guar gum): 0.7%

[0311] Steel fiber: 0.3%

[0312] Implementation steps:

[0313] Materials to be provided:

[0314] Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, fatty acid, guar gum and steel fiber.

[0315] Preparation of graphene suspension:

[0316] 0.8% graphene was dispersed in deionized water to form a graphene suspension.

[0317] Microencapsulation of phase change materials:

[0318] The fatty acid is heated to a molten state and then dissolved in an appropriate amount of an organic solvent to form a uniform solution.

[0319] Dissolve gelatin and gum arabic in warm water at 45°C respectively, stir evenly to form a composite wall material solution.

[0320] Slowly drip the fatty acid solution into the wall material solution while stirring, maintaining the temperature at 45°C and the stirring rate at 400 rpm.

[0321] The temperature of the mixed solution was lowered to 12°C, stirring was continued, and the pH value was adjusted to 4.2 to form microcapsules.

[0322] Solidification is performed by freeze drying, and the dried microcapsule fatty acid is collected and sieved to obtain a microcapsule phase change material with uniform particle size.

[0323] Dry mix base mixture:

[0324] Cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide are dry-mixed to form a basic mixture.

[0325] Wet mix base mixture:

[0326] The base mixture is wet-mixed with the graphene suspension and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed.

[0327] Add green high-efficiency water reducing agent:

[0328] During the wet mixing process, guar gum is gradually added to adjust the working properties of the mixture to ensure that the mixture has good fluidity and stability.

[0329] Adding steel fibers:

[0330] Add the steel fibers last and continue stirring until the steel fibers are evenly distributed.

[0331] Compaction with magnetorheological fluid technology:

[0332] The mixture is poured into a mold that has been pre-coated with a layer of magnetorheological fluid.

[0333] The electromagnetic coil was installed with an initial magnetic field strength of 0.5 T, a maximum magnetic field strength of 1 T, and a magnetic field application time of 10 minutes.

[0334] Different magnetic field intensities were applied in three stages, and the compaction effects of the magnetic field and the mixture were monitored in real time.

[0335] Demolding and wet curing after initial setting:

[0336] Demoulding is carried out after initial setting (within 24 hours).

[0337] The demoulded samples were placed in a wet curing box with the temperature set at 20°C and the humidity maintained at 95% for 7 days.

[0338] Carbon dioxide maintenance:

[0339] The samples after wet curing were moved into a carbon dioxide curing box, the temperature was set at 20°C, the carbon dioxide concentration was controlled at 15%, carbon dioxide curing was performed for 8 hours a day, and the rest of the time was kept in room temperature.

[0340] Cyclic heating:

[0341] Initial setting: The initial heating time is 1.5 hours, and the material temperature is gradually raised to the phase change temperature of the phase change material (50°C).

[0342] The heating cycle was set to once every 7.5 hours, with each heating time of 0.5 hours, and the temperature was maintained within the phase transition temperature range.

[0343] Cooling cycle setting: After each heating, perform natural cooling for 6.5 hours, monitor temperature changes, and the temperature should not be lower than room temperature.

[0344] High temperature sintering treatment:

[0345] After curing for 28 days, the samples were sintered at high temperature with the temperature set at 850°C for 3 hours.

[0346] Summary of Example 5:

[0347] On the basis of Example 4, the material ratio and the type of phase change material were optimized, guar gum was used as a green and efficient water reducer, and the parameters of magnetorheological fluid technology compaction and the temperature setting of periodic heating were further optimized, which significantly improved the overall performance and durability of the material.

[0348] Summary:

[0349] Based on the first embodiment, these five embodiments gradually adjust the material ratio and the type of phase change material, optimize the parameters of magnetorheological fluid technology compaction, improve the conditions of wet curing and carbon dioxide curing, and optimize the temperature and time settings of periodic heating. Each embodiment further develops on the basis of the previous one, demonstrating the influence of different material combinations and process parameters on material properties. Ultimately, through these optimization measures, the density, fluidity, stability, durability and overall performance of ultra-high performance cement-based materials mixed with waste glass powder are significantly improved, meeting the high-demand engineering application needs.

[0350] Experimental design:

[0351] Purpose:

[0352] Verify the improvements and advantages of the ultra-high performance cement-based material preparation method incorporating waste glass powder compared to the traditional preparation method in terms of density, fluidity, stability, durability and overall performance.

[0353] Experimental design:

[0354] The experimental comparison scheme includes:

[0355] Traditional preparation method

[0356] Embodiment 1 of the present invention

[0357] Embodiment 2 of the present invention

[0358] Embodiment 3 of the present invention

[0359] Embodiment 4 of the present invention

[0360] Embodiment 5 of the present invention

[0361] Experimental steps:

[0362] 1. Material preparation:

[0363] Traditional preparation method:

[0364] Cement, waste glass powder, silica fume, fine aggregate, steel fiber, water reducing agent.

[0365] Embodiments of the present invention:

[0366] Cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, phase change material (paraffin / fatty acid / hydrated salt), green and high-efficiency water reducer (tannic acid / guar gum / plant-based water reducer), and steel fiber.

[0367] 2.Material ratio:

[0368] Materials were prepared in the weight percentages specified in the respective Examples and Conventional Methods.

[0369] 3. Mixing and stirring:

[0370] Traditional method: Use ordinary mixing equipment to mix and ensure uniformity.

[0371] The method of the present invention:

[0372] Preparation of graphene suspension and microencapsulation of phase change materials.

[0373] Dry mix base mixture, wet mix base mixture, add water reducer and steel fiber.

[0374] Use a high shear mixer to mix until a homogeneous mixture is obtained.

[0375] 4. Mold filling and compaction:

[0376] Traditional method: The mixture is poured into a mold and compacted using mechanical vibration.

[0377] The method of the invention comprises the following steps: pouring the mixture into a mold and compacting the mixture by using magnetorheological fluid technology.

[0378] 5. Maintenance:

[0379] Traditional method: conventional wet curing for 28 days.

[0380] The method of the present invention:

[0381] Demould after initial setting and carry out wet curing for the first 7 days.

[0382] Carbon dioxide curing is carried out from the 8th day to the 28th day.

[0383] Periodic heating is carried out during curing.

[0384] After 28 days of curing, high temperature sintering treatment is carried out.

[0385] 6. Test items:

[0386] Density (porosity)

[0387] Fluidity (slump, expansion)

[0388] Stability (segregation test)

[0389] Durability (freeze-thaw resistance, penetration resistance)

[0390] Strength (compressive strength)

[0391] Table 1:

[0392]

[0393] Summarize:

[0394] By comparing the traditional preparation method with the five embodiments of the present invention, the performance of different methods in terms of density, fluidity, stability, durability and strength is comprehensively evaluated. The experimental data are shown in Table 1, and the specific analysis is as follows:

[0395] Density (porosity):

[0396] The porosity of the sample prepared by the traditional method is 15.2%, which is significantly higher than the porosity of each embodiment of the present invention.

[0397] The porosity of the embodiments of the present invention is lower than 10%. With the optimization of the process, the porosity is gradually reduced, and the lowest value of 9.1% is reached in the fifth embodiment.

[0398] Fluidity (slump, expansion):

[0399] The slump and spread of the traditional method are 180 mm and 500 mm respectively.

[0400] The slump and spread of each embodiment of the present invention are significantly improved. The slump and spread of embodiment 5 reach 230 mm and 585 mm respectively, indicating that the material has better fluidity.

[0401] Stability (segregation rate):

[0402] The separation rate of the traditional method is 5.8%, which is significantly higher than that of the embodiments of the present invention.

[0403] The segregation rates of all embodiments of the present invention are lower than 2.5%, and the segregation rate of Embodiment 5 is the lowest, which is only 1.5%, indicating that the material mixing is more uniform and the stability is better.

[0404] Durability (freeze-thaw resistance, penetration resistance):

[0405] The samples prepared by the traditional method can only resist 25 freeze-thaw cycles and the penetration depth is 22 mm.

[0406] The number of freeze-thaw cycles of each embodiment of the present invention is significantly improved, and the number of freeze-thaw cycles of embodiment 5 reaches 80 times.

[0407] The anti-penetration depth of each embodiment of the present invention is significantly reduced, and the anti-penetration depth of embodiment 5 is only 11 mm, indicating that the durability of the material is significantly improved.

[0408] Strength (compressive strength):

[0409] The compressive strength of the sample prepared by the traditional method is 80MPa.

[0410] The compressive strength of each embodiment of the present invention is significantly higher than that of the traditional method, and the fifth embodiment reaches the highest value of 140 MPa.

[0411] Summary

[0412] The experimental results clearly show that the method of the present invention is superior to the traditional method in various performance indicators, which are specifically manifested as follows:

[0413] The density is significantly improved and the porosity is greatly reduced.

[0414] The fluidity is significantly improved, and the slump and expansion are significantly increased.

[0415] The stability is greatly improved and the segregation rate is significantly reduced.

[0416] The durability is significantly enhanced, and the number of freeze-thaw cycles and anti-penetration performance are greatly improved.

[0417] The strength is significantly improved and the compressive strength is greatly increased.

[0418] In the previous experiment, by comparing the traditional preparation method with the method of the present invention, the significant advantages of the present invention in terms of material density, fluidity, stability, durability and overall performance were verified. The experimental results show that the method of the present invention using magnetorheological fluid technology, microencapsulated phase change material and carbon dioxide curing technology has obvious innovation and superiority in improving material performance and environmental protection.

[0419] In order to further explore the influence of different process parameters of the preparation method of the present invention on material properties. This experiment not only compares the influence of different magnetic field strengths, different phase change materials and different curing conditions on material properties, but also further analyzes the optimization effect of these parameter combinations in practical applications. Through in-depth research on these key parameters, the applicability and superiority of the present method under different conditions are comprehensively evaluated, providing a more scientific and comprehensive basis for the development of high-performance cement-based materials in the future.

[0420] Experimental design:

[0421] Purpose:

[0422] The performance of the ultra-high performance cement-based material preparation method of the present invention under different process parameters is deeply explored.

[0423] Experimental design:

[0424] The experimental comparison scheme includes:

[0425] Traditional preparation method:

[0426] The method of the present invention (standard process parameters)

[0427] Method of the present invention (different magnetic field strengths)

[0428] Method of the present invention (different phase change materials)

[0429] The method of the present invention (different curing conditions)

[0430] Experimental steps:

[0431] 1. Material Preparation

[0432] Traditional preparation method:

[0433] Cement, waste glass powder, silica fume, fine aggregate, steel fiber, water reducing agent.

[0434] The method of the present invention:

[0435] Cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, phase change material (paraffin / fatty acid / hydrated salt), green and high-efficiency water reducer (tannic acid / guar gum / plant-based water reducer), and steel fiber.

[0436] 2.Material ratio:

[0437] Materials were prepared in the weight percentages specified in the respective Examples and Conventional Methods.

[0438] 3. Mixing and stirring:

[0439] Traditional method: Use ordinary mixing equipment to mix and ensure uniformity.

[0440] The method of the present invention:

[0441] Preparation of graphene suspension and microencapsulation of phase change materials.

[0442] Dry mix base mixture, wet mix base mixture, add water reducer and steel fiber.

[0443] Use a high shear mixer to mix until a homogeneous mixture is obtained.

[0444] 4. Mold filling and compaction:

[0445] Traditional method: The mixture is poured into a mold and compacted using mechanical vibration.

[0446] The method of the invention comprises the following steps: pouring the mixture into a mold and compacting the mixture by using magnetorheological fluid technology.

[0447] 5. Maintenance:

[0448] Traditional method: conventional wet curing for 28 days.

[0449] The method of the present invention:

[0450] Demould after initial setting and carry out wet curing for the first 7 days.

[0451] Carbon dioxide curing is carried out from the 8th day to the 28th day.

[0452] Periodic heating is carried out during curing.

[0453] After 28 days of curing, high temperature sintering treatment is carried out.

[0454] 6. Experimental parameter settings:

[0455] Different magnetic field strengths: 0.3T, 0.5T, 0.7T, 0.9T

[0456] Different phase change materials: paraffin, fatty acids, hydrated salts

[0457] Different curing conditions: wet curing (28 days), carbon dioxide curing (7 days wet curing + 21 days carbon dioxide curing)

[0458] 7. Test items:

[0459] Density (porosity)

[0460] Fluidity (slump, expansion)

[0461] Stability (segregation test)

[0462] Durability (freeze-thaw resistance, penetration resistance) Strength (compressive strength)

[0463] Table 2:

[0464]

[0465]

[0466] Experimental summary:

[0467] By comparing the experimental results, the creativity and superiority of the preparation method of the present invention are further verified.

[0468] The specific performance is as follows:

[0469] Influence of magnetic field strength:

[0470] As the magnetic field intensity increases, the porosity gradually decreases and the material density increases.

[0471] At magnetic field strengths of 0.7T and 0.9T, the material exhibits optimal fluidity and stability.

[0472] The freeze-thaw resistance and penetration resistance are significantly improved at higher magnetic field strengths.

[0473] Different phase change materials:

[0474] The use of paraffin, fatty acids and hydrated salts as phase change materials significantly improves the performance of the materials.

[0475] Paraffin and fatty acid phase change materials excel in fluidity and stability.

[0476] Hydrated salt has good performance in anti-freeze-thaw and anti-penetration properties.

[0477] Different maintenance conditions:

[0478] CO2 curing is significantly superior to conventional wet curing, especially in terms of durability.

[0479] The samples wet-cured for 28 days were inferior to those cured with carbon dioxide in terms of compressive strength and freeze-thaw resistance.

[0480] The above results further demonstrate the remarkable advantages of the innovative processes adopted in the present invention, such as magnetorheological fluid technology, microencapsulated phase change material, carbon dioxide curing and periodic heating, in improving material properties.

[0481] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing ultra-high performance cement-based materials mixed with waste glass powder, characterized in that: The following steps are involved: S1. Provide cement, waste glass powder, silica fume, fine aggregate, nano titanium dioxide, graphene, phase change material, green high-efficiency water reducing agent and steel fiber; S2, dispersing graphene in deionized water to form a graphene suspension; S3, microencapsulating the phase change material; S4, dry-mixing cement, waste glass powder, silica fume, fine aggregate and nano-titanium dioxide to form a basic mixture; S5, wet mixing the base mixture, the graphene suspension, and the microencapsulated phase change material in a high shear mixer until a uniform mixture is formed; S6. Gradually add green high-efficiency water reducer during wet mixing to adjust the working performance of the mixture; S7, finally add steel fiber and continue stirring until the steel fiber is evenly distributed; S8, pouring the mixture into a mold and compacting it using magnetorheological fluid technology; S9. After initial setting, demoulding is performed and the sample is placed in a curing box for standard curing; S10, during the curing period, the phase change material is heated periodically to release energy and adjust the internal temperature of the material; S11. After curing for 28 days, the sample is subjected to high-temperature sintering treatment.

2. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: In the step S1, by weight percentage, cement is 50-70%, waste glass powder is 10-20%, silica fume is 5-15%, fine aggregate is 10-20%, nano titanium dioxide is 1-5%, graphene is 0.1-1%, phase change material is 1-5%, green high-efficiency water reducing agent is 0.5-2%, and steel fiber is 0.5-2%.

3. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: The phase change material is selected from paraffin, fatty acid or hydrated salt, and the green high-efficiency water reducer is selected from plant-based water reducer, tannic acid or guar gum.

4. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: The specific steps of microencapsulation treatment in step S3 include the following: S3.1, prepare phase change material solution: The solid phase change material is heated to a molten state, and then dissolved in an appropriate amount of water or an organic solvent to form a uniform solution; S3.

2. Prepare wall material solution: Take gelatin and gum arabic, dissolve them in warm water at a temperature of 40-50°C, stir evenly, and form a gelatin-gum arabic composite wall material solution; S3.3, mixing phase change material and wall material solution: slowly drip the phase change material solution into the wall material solution, stirring while adding, maintaining the temperature at 40-50°C, and the stirring rate at 300-500rpm; S3.4, forming microcapsules: lowering the temperature of the mixed solution to 10-15°C, stirring continuously, allowing the phase change material to gradually solidify to form microcapsules, and adjusting the pH value to 4.0-4.5 to promote coprecipitation and coating of microcapsule wall materials; S3.

5. Solidification and collection: solidify the formed microcapsules by freeze drying or spray drying, collect the dried microcapsules, and sieve them to obtain microcapsule phase change materials with uniform particle size.

5. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: The method for adjusting the working performance of the mixture in step S6 is to test the fluidity and stability of the mixture by slump test, expansion test and segregation test respectively, and adjust the amount of water reducing agent according to the test results. The method for adjusting the amount of water reducing agent is: If the fluidity is insufficient, increase the amount of water reducing agent; If the mixture segregates, reduce the amount of water reducer or increase the proportion of fine aggregate.

6. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: The periodic heating rule in step S10 is: Initial settings: Set the initial heating time to 1.5-2h, gradually raise the material temperature to the phase change temperature of the phase change material, and control the initial heating temperature to a high value within the phase change temperature range; Heating cycle setting: The heating cycle is set to 7.5-8h once, with each heating time of 0.5-1h. In each heating cycle, the temperature is kept within the phase change temperature range; Cooling cycle setting: After each heating, turn off the heating device and perform natural cooling for 6-7 hours. During the cooling cycle, monitor the temperature change, and the internal temperature of the material gradually drops but does not fall below room temperature; Monitoring and adjustment: Use temperature sensors to monitor the temperature inside and on the surface of the material in real time, record temperature data, analyze the temperature changes in each heating and cooling cycle, and adjust the heating time, power and cycle based on the data analysis results to keep the temperature within the phase change temperature range.

7. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 6, characterized in that: The initial heating temperature is controlled within the phase change temperature range with an accuracy of ±2°C.

8. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: The maintenance in step S10 specifically includes the following steps: Wet curing stage (first 7 days): Place the demoulded samples in a wet curing box; The temperature range of the wet curing box is set at 18-22°C, and the humidity is maintained at 90-100%; Wet curing was continued for 7 days, and the sample surface remained moist; Carbon dioxide curing stage (Day 8 to Day 28): Move the wet-cured samples into a carbon dioxide curing box; Set the temperature range of the curing box to 18-22°C and the carbon dioxide concentration to 10-20%; Carbon dioxide curing was performed for 6-10 hours every day, and the samples were kept at room temperature for the rest of the time.

9. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 1, characterized in that: The magnetorheological fluid technology compaction in step S8 specifically includes the following steps: Prepare the mold and mixture: Pour the mixture into a mold pre-coated with a layer of magnetorheological fluid; Install the electromagnetic coil: install the electromagnetic coil on the outer wall and bottom of the mold; Set the magnetic field parameters: initial magnetic field strength 0.1-0.5T, maximum magnetic field strength 0.5-1T, magnetic field application time 3-10min; Start magnetic field compaction: Apply different magnetic field strengths in three stages, from small to large, and monitor the compaction effect of the magnetic field and the mixture in real time through the control system to adjust the magnetic field strength and action time; Compaction completion and curing: After the magnetic field ends, the electromagnetic coil is turned off and the mold is left to stand for preliminary curing.

10. The method for preparing an ultra-high performance cement-based material mixed with waste glass powder according to claim 6, characterized in that: The phase change temperature ranges of the phase change materials paraffin, fatty acid or hydrated salt are respectively 20-60° C. for paraffin, 30-70° C. for fatty acid and 30-50° C. for hydrated salt.

Citation Information

Patent Citations

  • High-strength lightweight inorganic energy-saving insulating building material and preparation method thereof

    CN107840612A

  • Low-carbon cement concrete and preparation method thereof

    CN114873979A

  • A materials construction with PCM micro capsule and method for manufacturing same

    KR1020120019497A

Cited By

  • Solid-waste-based green high-performance concrete and preparation method thereof

    CN122036285A