All-solid waste cementing material as well as preparation method and application thereof
Through the all-solid waste cement prepared by the whole industrial solid waste, combined with tailings sand, the problem of cemented filling materials taking into account strength and fluidity is solved, and the effects of high backfill strength, good fluidity and low carbon and environmental protection are achieved. The defects of cement cementitious materials are avoided, and the effect of mine filling and solid waste resource utilization are improved.
Patent Information
- Application Number
- CN202411159515.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to take into account the strength and fluidity of existing cemented filling materials, and traditional cemented cemented materials lead to problems of poor filling strength and easy shrinkage.
All solid waste cement prepared by using all-industry solid waste, including slag powder, steel slag powder, fly ash, desulfurization gypsum, red mud and activation raw materials, combined with tailings sand as aggregate, prepared through specific proportions and treatment methods A cementitious material with high backfill strength, good fluidity and low carbon and environmental protection.
It achieves high backfill strength, good fluidity and low shrinkage, avoids high energy consumption and high pollution in cement production, improves the resource utilization of solid waste, meets the requirements of mine filling, and improves the stability of the backfill structure.
Smart Images

Figure BDA0005006036200000081
Abstract
Description
Technical Field
[0001] The invention relates to a full-solid waste binder and a preparation method and application thereof. Background Art
[0002] Cementitious backfilling is to pump the backfill slurry made of aggregate and cementitious materials into the underground goaf. The backfill slurry gradually forms a backfill body with a certain strength in the underground goaf. This method can achieve green mining, ensure mine safety, and play a very important role in the recovery of minerals under the mountain. Cementitious backfilling materials are mainly composed of aggregate and cementitious materials. There are two main problems facing cementitious backfilling at present. One is that using traditional cementitious materials such as cement as the cementing material will lead to poor filling strength and easy shrinkage in the cementing of the whole tailings. The second is that strength and fluidity cannot be taken into account at the same time.
[0003] CN114940600A discloses a full solid waste filling material and a preparation method thereof. The gel material includes desulfurized gypsum, fly ash, slag, steel slag, magnesium slag, carbide slag, water reducing agent, water retaining dispersant and alkaline activator; the aggregate is tailings. This patent utilizes the theory of synergistic complementation of multi-source solid waste chemical components, and the reaction generates stronger AFm crystals. The water retaining dispersant reasonably solves the segregation and water seepage problems of the full solid waste filling material, but does not disclose information related to self-flow and shrinkage.
[0004] CN116639945A discloses a method for preparing cementing filling materials by using multi-source industrial waste slag and ultra-fine tailings. The method comprises the following steps: S1. Drying steel slag, fly ash, carbide slag, desulfurized gypsum, and blast furnace slag, and then putting them into a ball mill to grind to a predetermined gradation, weighing the raw materials in proportion, and mixing them evenly to form an industrial solid waste-based cementing material; S2. Mixing ultra-fine tailings, industrial solid waste-based cementing materials with water, and stirring them evenly to obtain a cementing filling material; S3. Curing the prepared filling material under standard conditions for 3 days and 28 days to conduct a uniaxial compressive strength test to evaluate the performance of the cementing filling material. The main raw materials of this method include steel slag, fly ash, carbide slag, desulfurized gypsum, and blast furnace slag, all of which are solid waste products, but the proportion of cementing tailings is relatively low, and one part of cementing material can only cement 4 parts of tailings, and the patent does not disclose information related to fluidity and shrinkage. Summary of the invention
[0005] In view of this, one object of the present invention is to provide a full-solid waste binder, which is prepared from all industrial solid waste and has the characteristics of high backfill strength, good fluidity, not easy to shrink, low carbon and environmental protection. Another object of the present invention is to provide a method for preparing the full-solid waste binder as described above. Another object of the present invention is to provide an application of the full-solid waste binder as described above in mine backfill, mine filling, tailings solidification treatment or foundation backfill.
[0006] The above technical objectives are achieved through the following technical solutions.
[0007] On the one hand, the present invention provides an all-solid waste binder, including a cementitious material and tailings sand; wherein the cementitious material includes the following components in parts by weight: 30 to 80 parts of slag powder, 15 to 30 parts of steel slag powder, 10 to 25 parts of fly ash, 2 to 20 parts of desulfurized gypsum, 1 to 10 parts of red mud, and 3 to 10 parts of activated raw materials; the mass ratio of the cementitious material to the tailings sand is 1:8 to 13.
[0008] According to the all-solid waste binder of the present invention, preferably, the activation raw materials are selected from at least two of a water reducing enhancer, a strong alkali and a sulfate.
[0009] According to the all-solid waste binder of the present invention, preferably, the water reducing enhancer is selected from one or more of polycarboxylic acid water reducers, naphthalene-based water reducers, and lignin sulfonate water reducers.
[0010] According to the all-solid waste binder of the present invention, preferably, the activated raw material consists of a water reducing enhancer, a strong alkali and a sulfate; the activated raw material consists of a water reducing enhancer, a strong alkali and a sulfate; wherein the mass ratio of the water reducing enhancer: the strong alkali: the sulfate is 0.1-1:0.1-2:1-10.
[0011] According to the all-solid waste binder of the present invention, preferably, the desulfurized gypsum is obtained by flue gas desulfurization treatment; the specific surface area of the desulfurized gypsum is greater than 350m 2 / kg.
[0012] According to the all-solid waste binder of the present invention, preferably, the particle size of the tailings sand is ≤4.75 mm.
[0013] According to the all-solid waste binder of the present invention, preferably, the mass ratio of the cementitious material to the tailings sand is 1:10-12.
[0014] According to the all-solid waste binder of the present invention, preferably, the specific surface area of the slag powder is 500-650m 2 / kg; the specific surface area of steel slag powder is 400~550m 2 / kg; the specific surface area of the red mud is greater than 400m 2 / kg.
[0015] On the other hand, the present invention provides a method for preparing the all-solid waste binder as described above, comprising the following steps:
[0016] (1) uniformly mixing slag powder, steel slag powder, fly ash, desulfurized gypsum, red mud and activated raw materials to obtain a cementitious material;
[0017] (2) Weigh tailings sand according to the mass ratio of cementitious material to tailings sand, mix the cementitious material and tailings sand evenly, add water to obtain slurry, and stir the slurry evenly to obtain the all-solid waste binder.
[0018] On the other hand, the present invention provides a use of the all-solid waste binder as described above in mine backfill, mine filling, tailings solidification treatment or foundation backfill.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The present invention completely uses solid waste as the main raw material of the binder, combines it with activated raw materials, and uses tailings sand as aggregate. The resulting filling material can fully meet the requirements of mine filling.
[0021] (2) The present invention does not use cement, thus avoiding the high energy consumption and high pollution in cement production, and effectively improving the problems of poor strength and easy shrinkage caused by using cement as a filling binder.
[0022] (3) The resource utilization of solid waste has been improved, and tailings sand has been used as aggregate to solve the problem of large-scale accumulation of tailings. DETAILED DESCRIPTION
[0023] The present invention is described in more detail below, but the present invention is not limited thereto.
[0024] <All solid waste binder>
[0025] The all-solid waste binder of the present invention is prepared from a cementitious material and an aggregate, wherein the cementitious material includes slag powder, steel slag powder, fly ash, desulfurized gypsum, red mud and activated raw materials; and the tailings sand is used as the aggregate.
[0026] In the present invention, the slag powder can be selected from the slag powder in GB / T 18046-2017, preferably slag powder of grade S95 or above. The specific surface area of the slag powder can be 500 to 650 m 2 / kg, preferably 550-600m 2 The mass of the slag powder may be 30 to 80 parts, preferably 45 to 65 parts, and more preferably 50 to 55 parts.
[0027] In the present invention, the steel slag powder can be selected from the steel slag powder in GB / T 20491-2017, preferably first-grade steel slag powder. The specific surface area of the steel slag powder can be 400 to 550 m 2 / kg, preferably 450-500m 2 The weight of the steel slag powder may be 15 to 30 parts, preferably 18 to 28 parts, and more preferably 20 to 25 parts.
[0028] In the present invention, fly ash can be selected from the fly ash in GB / T 1596-2017, preferably F-type fly ash; more preferably F-type I fly ash with a particle size of 45 μm square hole sieve residue ≤12%; and more preferably F-type I fly ash with a particle size of 45 μm square hole sieve residue <10%. The mass of fly ash can be 10 to 25 parts, preferably 12 to 22 parts, and more preferably 15 to 20 parts.
[0029] In the present invention, the desulfurized gypsum can be obtained by flue gas desulfurization treatment, preferably by wet flue gas desulfurization treatment. The specific surface area of the desulfurized gypsum can be greater than 350m 2 / kg, preferably greater than 400m 2 / kg, more preferably greater than 450m 2 The mass of the desulfurized gypsum can be 2 to 20 parts, preferably 3 to 15 parts, and more preferably 5 to 10 parts.
[0030] In the present invention, red mud is industrial solid waste generated by the preparation of alumina, and can be sintered red mud, Bayer red mud or combined red mud, preferably sintered red mud. The specific surface area of red mud can be greater than 400m 2 / kg, preferably greater than 450m 2 / kg, more preferably greater than 500m 2 The mass of red mud may be 1 to 10 parts, preferably 2 to 7 parts, and more preferably 3 to 5 parts.
[0031] In the present invention, the activation raw material can be selected from at least two of a water-reducing enhancer, a strong base and a sulfate, preferably consisting of a water-reducing enhancer, a strong base and a sulfate. Among them, the water-reducing enhancer can be selected from one or more of a polycarboxylate water-reducer, a naphthalene water-reducer, and a lignin sulfonate water-reducer, preferably selected from a polycarboxylate water-reducer or a naphthalene water-reducer, more preferably a polycarboxylate water-reducer. The strong base can be an alkaline hydroxide, can be selected from one or more of potassium hydroxide, sodium hydroxide, and calcium hydroxide, preferably potassium hydroxide or sodium hydroxide, more preferably sodium hydroxide. The sulfate can be selected from one or more of sodium sulfate, potassium sulfate, and calcium sulfate, preferably sodium sulfate or potassium sulfate, more preferably sodium sulfate.
[0032] In the present invention, the mass ratio of water reducing enhancer: strong base: sulfate can be 0.1-1: 0.1-2: 1-10; preferably, the mass ratio of water reducing enhancer: strong base: sulfate is 0.2-0.7: 0.5-1.5: 2-8; more preferably, the mass ratio of water reducing enhancer: strong base: sulfate is 0.3-0.5: 0.8-1.2: 3-6.
[0033] In the present invention, the particle size of the tailings may be 4.75 mm or less, preferably 2.8 mm or less, and more preferably 2 mm or less. The mass ratio of the cementitious material to the tailings may be 1:8-13, preferably 1:9-12, and more preferably 1:10-11.
[0034] <Preparation method of all-solid waste binder>
[0035] The preparation method of the all-solid waste binder of the present invention comprises the following steps:
[0036] The slag powder, steel slag powder, fly ash, desulfurized gypsum, red mud and activated raw materials are uniformly mixed to obtain the cementitious material.
[0037] The tailings sand is weighed according to the mass ratio of the cementitious material to the tailings sand, and the cementitious material and the tailings sand are evenly mixed, and then water is added to obtain a slurry, and the slurry is stirred evenly to obtain the all-solid waste binder.
[0038] In the present invention, the water is preferably untreated tap water; the mass concentration of the slurry may be 65-85%, preferably 70-85%, and more preferably 75-82%.
[0039] In the present invention, there is no special regulation on the mixing method, and the commonly used methods in the art can be used, such as mechanical stirring.
[0040] <Application of all-solid waste binder>
[0041] The all-solid waste binder of the present invention can be used in mine backfill, mine filling, foundation backfill, and can also be used in ecological environment management, such as solidification treatment of tailings; preferably used in mine backfill.
[0042] In the following examples, unless otherwise specified, the parts are by weight.
[0043] Example 1
[0044] 50 parts of slag powder, 20 parts of steel slag powder, 18 parts of fly ash, 9 parts of desulfurized gypsum, 3 parts of red mud, 4 parts of sodium sulfate, 0.8 parts of sodium hydroxide, and 0.3 parts of polycarboxylate water reducer are mixed evenly to obtain a cementitious material. The specific surface area of the slag powder is 500m 2 / kg, the specific surface area of steel slag powder is 450m 2 / kg, the fly ash is Class F I fly ash with a 45μm square hole sieve residue of ≤12%, and the specific surface area of desulfurized gypsum is 400m 2 / kg, the specific surface area of red mud is 450m 2 / kg.
[0045] Weigh tailings sand according to the mass ratio of cementitious material to tailings sand (as aggregate) of 1:10; mix the cementitious material and tailings sand weighed above, add water to obtain a slurry with a concentration of 76%, and stir evenly in a mixer to obtain a full-solid waste binder.
[0046] Example 2
[0047] 55 parts of slag powder, 23 parts of steel slag powder, 16 parts of fly ash, 4 parts of desulfurized gypsum, 2 parts of red mud, 6 parts of sodium sulfate, 1 part of sodium hydroxide and 0.4 parts of polycarboxylic acid water reducer were uniformly mixed to obtain a cementitious material.
[0048] Weigh tailings sand according to a mass ratio of cementitious material to tailings sand of 1:12; mix the cementitious material and tailings sand weighed above, add water to obtain a slurry with a concentration of 78%, and stir evenly in a mixer to obtain a full-solid waste binder.
[0049] Example 3
[0050] 45 parts of slag powder, 25 parts of steel slag powder, 18 parts of fly ash, 7 parts of desulfurized gypsum, 5 parts of red mud, 5 parts of sodium sulfate, 1.2 parts of sodium hydroxide and 0.3 parts of polycarboxylic acid water reducer were uniformly mixed to obtain a cementitious material.
[0051] Weigh tailings sand according to a mass ratio of cementitious material to tailings sand of 1:10; mix the cementitious material and tailings sand weighed above, add water to obtain a slurry with a concentration of 82%, and stir evenly in a mixer to obtain a full-solid waste binder.
[0052] Example 4
[0053] 50 parts of slag powder, 23 parts of steel slag powder, 15 parts of fly ash, 10 parts of desulfurized gypsum, 2 parts of red mud, 5 parts of sodium sulfate, 1 part of sodium hydroxide and 0.4 parts of polycarboxylic acid water reducer were uniformly mixed to obtain a cementitious material.
[0054] Weigh tailings sand according to a mass ratio of cementitious material to tailings sand of 1:10; mix the weighed cementitious material and tailings sand, add water to obtain a slurry with a concentration of 80%, and stir evenly in a mixer to obtain a full-solid waste binder.
[0055] Example 5
[0056] 55 parts of slag powder, 20 parts of steel slag powder, 20 parts of fly ash, 3 parts of desulfurized gypsum, 2 parts of red mud, 5 parts of sodium sulfate, 1 part of sodium hydroxide and 0.4 parts of polycarboxylic acid water reducer were uniformly mixed to obtain a cementitious material.
[0057] Weigh tailings sand according to a mass ratio of cementitious material to tailings sand of 1:10; mix the cementitious material and tailings sand weighed above, add water according to a slurry concentration of 80%, and stir evenly in a mixer to obtain a full-solid waste binder.
[0058] Comparative Example 1
[0059] Except that the cementitious material is 100 parts of P.O42.5 cement, the rest is the same as Example 1.
[0060] Comparative Example 2
[0061] Except that sodium sulfate, sodium hydroxide and polycarboxylate water reducer are not added and desulfurized gypsum is replaced by anhydrous gypsum, the rest is the same as Example 1.
[0062] The slurries obtained in Examples 1 to 5 and Comparative Examples 1 to 2 were cast and cured to different ages for compressive strength tests, and the test method was based on the method in JC / T 2468-2018 "Cement-based Backfill Materials". The test results are shown in Table 1.
[0063] Table 1
[0064]
[0065] From the results in Table 1, it can be seen that the all-solid waste binder provided by the present invention has good compressive strength, the compressive strength after curing for 28 days is greater than 2MPa, the fluidity is greater than 200mm, and the 28d shrinkage rate is less than 0.1%, which meets the requirements of mine filling. At the same time, the smaller shrinkage rate makes the volume change of the backfill material smaller, which can effectively reduce the deformation and cracking problems after backfilling, thereby improving the stability and integrity of the backfill structure. Without using cement as a cementitious material, a binder with both strength and fluidity can be prepared by using solid waste raw materials and activated raw materials in combination.
[0066] In comparative example 1, the cementitious material was replaced with cement in equal amounts, and the 28d strength of the prepared binder was 1.75MPa, and the 28d shrinkage was relatively large. In comparative example 2, anhydrous gypsum was used without adding activated raw materials, and the 28d strength was 2.95MPa, which met the strength requirements, but the fluidity was only 160mm, and it did not have self-flowing properties.
[0067] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A solid waste binder, characterized in that: It includes cementitious material and tailings sand; wherein the cementitious material includes the following components in parts by weight: 30 to 80 parts of slag powder, 15 to 30 parts of steel slag powder, 10 to 25 parts of fly ash, 2 to 20 parts of desulfurized gypsum, 1 to 10 parts of red mud, and 3 to 10 parts of activated raw materials; the mass ratio of the cementitious material to the tailings sand is 1:8 to 13.
2. The all-solid waste binder according to claim 1, characterized in that: The activation raw materials are selected from at least two of a water reducing enhancer, a strong base and a sulfate.
3. The all-solid waste binder according to claim 2, characterized in that: The water reducing enhancer is selected from one or more of polycarboxylate water reducing agent, naphthalene water reducing agent and lignin sulfonate water reducing agent.
4. The all-solid waste binder according to claim 2, characterized in that: The activation raw material consists of a water reducing enhancer, a strong base and a sulfate; wherein the mass ratio of the water reducing enhancer: the strong base: the sulfate is 0.1-1: 0.1-2: 1-10.
5. The all-solid waste binder according to claim 1, characterized in that: The desulfurized gypsum is obtained by flue gas desulfurization treatment; the specific surface area of the desulfurized gypsum is greater than 350m 2 / kg.
6. The all-solid waste binder according to claim 1, characterized in that: The particle size of the tailings sand is ≤4.75mm.
7. The all-solid waste binder according to claim 1, characterized in that: The mass ratio of the gelling material to the tailings sand is 1:10-12.
8. The all-solid waste binder according to claim 1, characterized in that: The specific surface area of the slag powder is 500-650m 2 / kg; the specific surface area of steel slag powder is 400~550m 2 / kg; the specific surface area of the red mud is greater than 400m 2 / kg.
9. A method for preparing a solid waste binder according to any one of claims 1 to 8, characterized in that: The steps include: (1) uniformly mixing slag powder, steel slag powder, fly ash, desulfurized gypsum, red mud and activated raw materials to obtain a cementitious material; (2) Weigh tailings sand according to the mass ratio of cementitious material to tailings sand, mix the cementitious material and tailings sand evenly, add water to obtain slurry, and stir the slurry evenly to obtain the all-solid waste binder.
10. Use of the all-solid waste binder as claimed in any one of claims 1 to 8 or the all-solid waste binder obtained by the preparation method according to claim 9 in mine backfill, mine filling, tailings solidification treatment or foundation backfill.
Citation Information
Cited By
All-solid waste cementing material and preparation method thereof
CN119822776A
A fully solid waste cementitious material and its preparation method
CN119822776B
Steel and iron slag composite cementing material containing red mud and preparation method of steel and iron slag composite cementing material
CN121361979A