High-strength concrete and preparation method thereof

Through the combined use of modified regenerated coarse aggregate and boron-titanium modified carbon fiber, the problem of insufficient performance of existing regenerated concrete is solved, the mechanical properties and durability of high-strength concrete are significantly improved, the resource utilization of construction waste has been promoted, and the resource utilization of construction waste has been achieved. Efficient regeneration of building materials.

CN118930195AActive Publication Date: 2024-11-12TIANYUAN CONSTR GROUP +1

Patent Information

Application Number
CN202411225235.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The poor compressive strength, durability and stability of recycled concrete in the prior art limits its wide application in the construction field, and the resource utilization rate of construction waste is low, so a method that can effectively improve the performance of recycled aggregates is needed.

Method used

Modified regenerated crude aggregate is used in combination with boron-titanium modified carbon fiber, and the hydrophobicity and mechanical properties of the regenerated aggregate are improved through modified silicon sol treatment and nanomaterial blending, and high-strength concrete is prepared through specific process flow.

Benefits of technology

It significantly improves the mechanical properties and durability of high-strength concrete, enhances compressive strength, bending strength and permeability, provides higher resource utilization rate of construction waste, and has good social and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930195A_ABST
    Figure CN118930195A_ABST
Patent Text Reader

Abstract

The invention discloses high-strength concrete and a preparation method thereof, and belongs to the technical field of building materials. The concrete is prepared from the following raw materials in parts by weight: 50-80 parts of modified recycled coarse aggregate, 100-120 parts of fine aggregate, 160-200 parts of cement, 10-30 parts of a fiber reinforcing agent, 5-8 parts of a water reducing agent and 180-200 parts of water, the fiber reinforcing agent is boron-titanium modified carbon fiber. The construction waste is modified to obtain the coarse aggregate, the boron-titanium modified carbon fiber is used as a reinforcing agent, the coarse aggregate and the boron-titanium modified carbon fiber have a synergistic effect to achieve the effect of enhancing the mechanical property of the concrete, meanwhile, the reutilization rate of the construction waste is increased, and good economic benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to high-strength concrete and a preparation method thereof. Background Art

[0002] Concrete is one of the main materials in the construction industry and the backbone material of buildings. High-strength concrete refers to concrete with a strength grade of C60 or above. It is made of cement, sand, stone raw materials and water reducer, or fly ash, mineral powder, slag, silica powder and other mixtures, and is produced by conventional processes to obtain high-strength concrete. As a new building material, high-strength concrete is widely used in high-rise building structures, long-span bridge structures and some special structures due to its high compressive strength, strong deformation resistance, high density and low porosity. The biggest feature of high-strength concrete is its high compressive strength, which is generally 46 times that of ordinary strength concrete, so it can reduce the cross-section of components, making it most suitable for high-rise buildings.

[0003] In recent years, the construction industry, as one of the pillar industries of my country's national economy, has always maintained rapid development, and the urbanization process has continued to accelerate. With the continuous increase in the urbanization process, more and more old communities and rural self-built houses have been demolished, resulting in a large amount of abandoned construction waste. The solid waste generated by the demolition of buildings in my country has exceeded 2 trillion tons each year. This figure will continue to increase with the rapid development of the infrastructure industry. A large number of abandoned concrete from the demolition of buildings and unqualified concrete produced by commercial concrete mixing stations are piled up in suburban open spaces, occupying a large amount of arable land and causing certain pollution to the environment. In terms of the resource utilization of construction waste, the resource utilization rate of construction waste in my country is only 5%, far lower than South Korea's 97%, so the resource utilization of construction waste needs to be solved urgently. Abandoned concrete after the demolition of buildings is one of the difficult problems that hinder the sustainable development of building materials. In the prior art, recycled aggregates are usually obtained by mechanically crushing and screening construction waste concrete after removing impurities such as steel bars. The recycled aggregates obtained by this method are inferior to natural aggregates in performance, such as low strength, many microcracks, low apparent density, and high water absorption, which makes recycled concrete inferior in compressive strength, durability and other properties, and limits the promotion and use of recycled concrete to a certain extent. Studies have found that by modifying recycled aggregates and pre-treating recycled aggregates with nanomaterials or high-quality mineral admixtures before use, the performance of recycled aggregates can be effectively improved, the transition zone between cement paste and aggregates can be optimized, and the performance of recycled concrete can be improved. Although there are many methods for modifying recycled concrete aggregates, the mechanical properties, durability and stability of concrete prepared using modified recycled aggregates vary greatly. Therefore, there is an urgent need to develop a high-strength concrete with good stability and durability. Summary of the invention

[0004] The purpose of the present invention is to provide a high-strength concrete, in which modified recycled coarse aggregate is used in combination with a boron-titanium modified carbon fiber reinforcement, and the concrete prepared by mixing with other raw materials has excellent mechanical properties and good application prospects.

[0005] In order to achieve the above technical objectives, the technical solution adopted by the present invention is: A high-strength concrete is made of the following raw materials in parts by weight: 50-80 parts of modified recycled coarse aggregate, 100-120 parts of fine aggregate, 160-200 parts of cement, 10-30 parts of fiber reinforcement, 5-8 parts of water reducer, and 180-200 parts of water; the fiber reinforcement is boron-titanium modified carbon fiber.

[0006] Preferably, the modified recycled coarse aggregate has a particle size of 5-30 mm.

[0007] Preferably, the modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in the modified silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

[0008] Preferably, the modified silica sol is prepared by the following method: take 50g of alkaline silica sol, add glacial acetic acid to adjust the pH value of the silica sol solution to 5.5 while magnetically stirring at a speed of 300r / min, then add 14.5g of dimethyldimethoxysilane, adjust the speed to 600r / min, stir the reaction for 1h, and then let it stand for 10h to obtain the modified silica sol.

[0009] Preferably, the alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.5.

[0010] Preferably, the boron-titanium modified carbon fiber is prepared by the following method: (1) Place the carbon fiber in a vacuum furnace, set the vacuum degree at 0.05 Pa, then heat it to 500 °C and keep it for 2 h, and then cool it naturally to obtain the pretreated carbon fiber; (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

[0011] Preferably, in step (1), the length of the carbon fiber is 5-10 mm.

[0012] Preferably, the fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0013] Preferably, the water reducer is a polycarboxylic acid-based high-efficiency water reducer.

[0014] The present invention also provides a method for preparing the above-mentioned high-strength concrete, which comprises the following steps: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in the present invention is ordinary Portland cement.

[0015] Nano-silica sol has high specific surface energy, high activation, nucleation and other characteristics. When added to cement-based materials, it can significantly enhance hydration activity and accelerate the hydration reaction rate. The extremely small nano-particle size allows it to physically fill the pores and cracks on the surface of recycled aggregates, thereby achieving the effect of enhancing the mechanical properties of the concrete substrate. However, nano-silica sol with high specific surface energy is very easy to agglomerate. Excessive addition will still cause the strength of recycled aggregate concrete to only decrease instead of increase. How to evenly add it to recycled aggregate concrete and how to select the appropriate dosage are the key points of nano-silica sol to improve the performance of recycled aggregate concrete. The present invention adopts dimethyldimethoxysilane to modify the silica sol, which can enhance the stability and dispersibility of the silica sol and prevent the silica sol from agglomerating. When the recycled coarse aggregate is immersed in the modified silica sol, the nanoparticles can be better filled into the pores of the aggregate, thereby obtaining the modified recycled coarse aggregate with a denser structure. At the same time, since the hydrophobicity of the recycled coarse aggregate after being treated with the modified silica sol is enhanced, the water absorption rate of the modified recycled coarse aggregate can be significantly reduced, thereby effectively preventing the occurrence of ion erosion caused by absorbing too much water, and improving the durability of the concrete.

[0016] The fiber reinforcement used in the present invention is boron-titanium modified carbon fiber, which uses dopamine hydrochloride to coat the surface of the carbon fiber to form a uniform carbon film, and at the same time uses a boron-titanium nanolayer prepared by a sol-gel method to evenly coat the surface of the carbon fiber. Compared with the unmodified carbon fiber, the surface of the carbon fiber coated with the boron-titanium nanolayer is significantly smoother ( Figure 1 As shown in the figure), the special surface energy of nanomaterials is used to enhance the interfacial bonding energy of carbon fiber and other concrete materials, which is conducive to the formation of more stable concrete materials; at the same time, the modified carbon fiber has the characteristics of high strength, high modulus, and high chemical stability, which can effectively improve the mechanical properties and durability of concrete. The obtained boron-titanium modified carbon fiber is used in combination with modified recycled coarse aggregate to effectively improve the bonding strength between old cement mortar and new cement mortar and reduce the water absorption rate and porosity of recycled aggregate, thereby reducing the weak interface generated inside the concrete when the recycled aggregate is used. At the same time, boron-titanium modified carbon fiber can enhance the interfacial bonding force between carbon fiber and concrete matrix, significantly improve the tensile strength, flexural strength and compressive strength of concrete, and improve the overall performance of concrete materials.

[0017] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention uses waste construction waste to prepare modified recycled coarse aggregate, thereby improving the utilization rate of construction waste, providing more channels for the resource utilization of construction waste, and having good social, environmental and economic benefits.

[0018] (2) The present invention combines modified recycled coarse aggregate with a fiber reinforcement agent to produce a high-strength concrete with excellent mechanical properties, good impermeability, and good durability, and has broad market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The SEM images are of the surface morphology of the fiber reinforcement used in the present invention before and after modification, wherein a) is the carbon fiber before modification, and b) is the boron-titanium modified carbon fiber after modification. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.

[0021] Example 1 A high-strength concrete is made of the following raw materials in parts by weight: 50kg of modified recycled coarse aggregate, 100kg of fine aggregate, 160kg of cement, 10kg of fiber reinforcement, 5kg of water reducer, and 180kg of water; the fiber reinforcement is boron-titanium modified carbon fiber. The particle size of the modified recycled coarse aggregate is 5-30mm.

[0022] The modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in the modified silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

[0023] The modified silica sol is prepared by the following method: 50 g of alkaline silica sol is taken, and glacial acetic acid is added while magnetically stirring at a speed of 300 r / min to adjust the pH value of the silica sol solution to 5.5, and then 14.5 g of dimethyldimethoxysilane is added thereto, and the speed is adjusted to 600 r / min, and the stirring reaction is carried out for 1 hour, and then the modified silica sol is allowed to stand for 10 hours to obtain the modified silica sol.

[0024] The alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.5.

[0025] The boron-titanium modified carbon fiber is prepared by the following method: (1) placing carbon fiber in a vacuum furnace, setting the vacuum degree at 0.05 Pa, then heating to 500° C. and keeping the temperature for 2 hours, and naturally cooling to obtain pretreated carbon fiber; the carbon fiber has a length of 5-10 mm; (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

[0026] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0027] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0028] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this embodiment is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0029] Example 2 A high-strength concrete is made from the following raw materials in parts by weight: 80 kg of modified recycled coarse aggregate, 120 kg of fine aggregate, 200 kg of cement, 30 kg of fiber reinforcement, 8 kg of water reducer, and 200 kg of water; the fiber reinforcement is boron-titanium modified carbon fiber.

[0030] The modified recycled coarse aggregate has a particle size of 5-30 mm.

[0031] The modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in the modified silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

[0032] The modified silica sol is prepared by the following method: 50 g of alkaline silica sol is taken, and glacial acetic acid is added while magnetically stirring at a speed of 300 r / min to adjust the pH value of the silica sol solution to 5.5, and then 14.5 g of dimethyldimethoxysilane is added thereto, and the speed is adjusted to 600 r / min, and the stirring reaction is carried out for 1 hour, and then the modified silica sol is allowed to stand for 10 hours to obtain the modified silica sol.

[0033] The alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.5.

[0034] The boron-titanium modified carbon fiber is prepared by the following method: (1) placing carbon fiber in a vacuum furnace, setting the vacuum degree at 0.05 Pa, then heating to 500° C. and keeping the temperature for 2 hours, and naturally cooling to obtain pretreated carbon fiber; the carbon fiber has a length of 5-10 mm; (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

[0035] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0036] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0037] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this embodiment is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0038] Example 3 A high-strength concrete is made of the following raw materials in parts by weight: 70kg of modified recycled coarse aggregate, 110kg of fine aggregate, 180kg of cement, 20kg of fiber reinforcement, 7kg of water reducer, and 190kg of water; the fiber reinforcement is boron-titanium modified carbon fiber.

[0039] The modified recycled coarse aggregate has a particle size of 5-30 mm.

[0040] The modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in the modified silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

[0041] The modified silica sol is prepared by the following method: 50 g of alkaline silica sol is taken, and glacial acetic acid is added while magnetically stirring at a speed of 300 r / min to adjust the pH value of the silica sol solution to 5.5, and then 14.5 g of dimethyldimethoxysilane is added thereto, and the speed is adjusted to 600 r / min, and the stirring reaction is carried out for 1 hour, and then the modified silica sol is allowed to stand for 10 hours to obtain the modified silica sol.

[0042] The alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.5.

[0043] The boron-titanium modified carbon fiber is prepared by the following method: (1) placing carbon fiber in a vacuum furnace, setting the vacuum degree at 0.05 Pa, then heating to 500° C. and keeping the temperature for 2 hours, and naturally cooling to obtain pretreated carbon fiber; the carbon fiber has a length of 5-10 mm; (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

[0044] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0045] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0046] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this embodiment is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0047] Comparative Example 1 A high-strength concrete is made from the following raw materials in parts by weight: 70 kg of modified recycled coarse aggregate, 110 kg of fine aggregate, 180 kg of cement, 20 kg of fiber reinforcement, 7 kg of water reducer, and 190 kg of water; the fiber reinforcement is boron-titanium modified carbon fiber.

[0048] The modified recycled coarse aggregate has a particle size of 5-30 mm.

[0049] The modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in an alkaline silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

[0050] The alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.5.

[0051] The boron-titanium modified carbon fiber is prepared by the following method: (1) placing carbon fiber in a vacuum furnace, setting the vacuum degree at 0.05 Pa, then heating to 500° C. and keeping the temperature for 2 hours, and naturally cooling to obtain pretreated carbon fiber; the carbon fiber has a length of 5-10 mm; (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

[0052] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0053] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0054] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this comparative example is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0055] This comparative example is the same as Example 3 except that unmodified silica sol is used in the preparation process of the modified recycled coarse aggregate.

[0056] Comparative Example 2 A high-strength concrete is made of the following raw materials in parts by weight: 70kg of modified recycled coarse aggregate, 110kg of fine aggregate, 180kg of cement, 20kg of fiber reinforcement, 7kg of water reducer, and 190kg of water; the fiber reinforcement is carbon fiber; and the length of the carbon fiber is 5-10mm.

[0057] The modified recycled coarse aggregate has a particle size of 5-30 mm.

[0058] The modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in the modified silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

[0059] The modified silica sol is prepared by the following method: 50 g of alkaline silica sol is taken, and glacial acetic acid is added while magnetically stirring at a speed of 300 r / min to adjust the pH value of the silica sol solution to 5.5, and then 14.5 g of dimethyldimethoxysilane is added thereto, and the speed is adjusted to 600 r / min, and the stirring reaction is carried out for 1 hour, and then the modified silica sol is allowed to stand for 10 hours to obtain the modified silica sol.

[0060] The alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.5.

[0061] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0062] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0063] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this embodiment is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0064] This comparative example is the same as Example 3 except that the fiber reinforcement is carbon fiber.

[0065] Comparative Example 3 A high-strength concrete is made from the following raw materials in parts by weight: 70 kg of recycled coarse aggregate, 110 kg of fine aggregate, 180 kg of cement, 20 kg of fiber reinforcement, 7 kg of water reducer, and 190 kg of water; the fiber reinforcement is boron-titanium modified carbon fiber.

[0066] The particle size of the recycled coarse aggregate is 5-30 mm.

[0067] The recycled coarse aggregate is prepared by the following method: waste concrete blocks are removed of impurities, placed in a muffle furnace, heated to 600° C., calcined for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain the recycled coarse aggregate.

[0068] The boron-titanium modified carbon fiber is prepared by the following method: (1) The carbon fiber is placed in a vacuum furnace, the vacuum degree is set at 0.05 Pa, and then the temperature is raised to 500° C. and kept at this temperature for 2 hours, and then naturally cooled to obtain pretreated carbon fiber; the length of the carbon fiber is 5-10 mm.

[0069] (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

[0070] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0071] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0072] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing recycled coarse aggregate and fiber reinforcement respectively; (2) Evenly mixing recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this embodiment is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0073] This comparative example is the same as Example 3 except that the modified recycled coarse aggregate and the preparation method are replaced by recycled coarse aggregate and the preparation method.

[0074] Comparative Example 4 A high-strength concrete is made of the following raw materials in parts by weight: 70kg recycled coarse aggregate, 110kg fine aggregate, 180kg cement, 20kg fiber reinforcement, 7kg water reducer, and 190kg water; the fiber reinforcement is carbon fiber; the length of the carbon fiber is 5-10mm; the particle size of the recycled coarse aggregate is 5-30mm.

[0075] The recycled coarse aggregate is prepared by the following method: waste concrete blocks are removed of impurities, placed in a muffle furnace, heated to 600° C., calcined for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain the recycled coarse aggregate.

[0076] The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:1.

[0077] The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

[0078] The preparation method of the above-mentioned high-strength concrete is as follows: (1) preparing recycled coarse aggregate and fiber reinforcement respectively; (2) Evenly mixing recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing. The cement used in this embodiment is PO 42.5 ordinary Portland cement produced by Shandong Linyi Yizhou Cement Co., Ltd.

[0079] This comparative example is the same as Example 3 except that unmodified silica sol is used in the preparation process of the modified recycled coarse aggregate.

[0080] Performance Testing The high-strength concrete prepared in Examples 1-3 and Comparative Examples 1-4 was cured for 28 days under the same temperature and humidity conditions and then subjected to mechanical property tests. The specific test methods were in accordance with GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete"; the concrete freeze-thaw test was carried out according to the quick freezing method in the "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete" (GB / T50082-2009), and the mass loss rate and compressive strength of the concrete samples after 400 freeze-thaw cycles were tested respectively. The results are shown in Table 1 below.

[0081] Table 1 Performance test results It can be seen from the data in Table 1 above that the high-strength concrete prepared by the present invention has significantly better compressive strength, flexural strength, splitting tensile strength, impermeability grade and freeze-thaw resistance than comparative examples 1-4, which indicates that the raw material components in the high-strength concrete of the present invention interact with each other, and the nanoparticles in the modified recycled aggregate can be better filled into the pores of the aggregate to obtain a modified recycled coarse aggregate with a denser structure; and the hydrophobicity of the modified recycled coarse aggregate is enhanced, which can significantly reduce the water absorption rate of the modified recycled coarse aggregate, thereby effectively preventing the occurrence of ion erosion caused by absorbing too much water, and improving the durability of the concrete. The modified recycled coarse aggregate is used in combination with boron-titanium modified carbon fiber and then mixed with other raw materials to prepare high-strength concrete with good performance. Changing any one of the raw material composition or dosage in the raw material formula cannot achieve the same technical effect.

[0082] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. A high-strength concrete, characterized in that: It is made of the following raw materials in parts by weight: 50-80 parts of modified recycled coarse aggregate, 100-120 parts of fine aggregate, 160-200 parts of cement, 10-30 parts of fiber reinforcement, 5-8 parts of water reducer and 180-200 parts of water; the fiber reinforcement is boron-titanium modified carbon fiber.

2. The high-strength concrete according to claim 1, characterized in that: The modified recycled coarse aggregate has a particle size of 5-30 mm.

3. The high-strength concrete according to claim 2, characterized in that: The modified recycled coarse aggregate is prepared by the following method: (a) After removing the debris from the waste concrete blocks, the waste concrete blocks are placed in a muffle furnace and heated to 600°C for calcination for 1 hour, then naturally cooled to room temperature, and crushed and ground to obtain pre-treated recycled coarse aggregate; (b) The pretreated recycled coarse aggregate is soaked in the modified silica sol solution for 6 hours, taken out, and dried in an oven at 120° C. for 2 hours to obtain the modified recycled coarse aggregate.

4. The high-strength concrete according to claim 3, characterized in that: The modified silica sol is prepared by the following method: 50 g of alkaline silica sol is taken, and glacial acetic acid is added while magnetically stirring at a speed of 300 r / min to adjust the pH value of the silica sol solution to 5.5, and then 14.5 g of dimethyldimethoxysilane is added thereto, and the speed is adjusted to 600 r / min, and the stirring reaction is carried out for 1 hour, and then the modified silica sol is allowed to stand for 10 hours to obtain the modified silica sol.

5. The high-strength concrete according to claim 4, characterized in that: The alkaline silica sol has a nano-silicon dioxide content of 30%, a particle size of 50-80 nm, and a pH of 8-8.

5.

6. The high-strength concrete according to claim 1, characterized in that: The boron-titanium modified carbon fiber is prepared by the following method: (1) Place the carbon fiber in a vacuum furnace, set the vacuum degree at 0.05 Pa, then heat it to 500 °C and keep it for 2 h, and then cool it naturally to obtain the pretreated carbon fiber; (2) adding 1 g of dopamine hydrochloride and 1.35 g of tris(hydroxymethyl)aminomethane to 1 L of deionized water to prepare a solution, and then immersing the pretreated carbon fiber obtained in step (1) therein, taking it out after 2 hours, and placing it in an oven and drying it at 60° C. for 24 hours to obtain a carbon nanolayer-coated carbon fiber; (3) Mix 3 ml of anhydrous ethanol with 1 ml of deionized water, and adjust the pH of the solution to 3.0 with nitric acid to obtain a mixed solution A; (4) Add 1 g of tetrabutyl titanate and 0.2 g of acetylacetone to 6 ml of anhydrous ethanol and disperse by ultrasonic for 5 min to obtain a mixed solution B; (5) Slowly pour the mixed solution A into the mixed solution B under magnetic stirring, then add 1.3 g of ammonium pentaborate and stir until it is completely dissolved to obtain a uniform sol solution; (6) The carbon fiber coated with the carbon nanolayer obtained in step (2) is immersed in the sol obtained in step (5), and after ultrasonic treatment for 10-15 minutes, it is taken out and dried completely in an oven, and then transferred to a vacuum furnace, heated to 1300° C. at 0.05 Pa, and kept warm for 90 minutes to obtain boron-titanium modified carbon fiber.

7. The high-strength concrete according to claim 6, characterized in that: In the step (1), the length of the carbon fiber is 5-10 mm.

8. The high-strength concrete according to claim 1, characterized in that: The fine aggregate is composed of machine-made river sand and slag in a mass ratio of 1:

1.

9. The high-strength concrete according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.

10. A method for preparing high-strength concrete according to any one of claims 1 to 9, characterized in that: It includes the following steps: (1) preparing modified recycled coarse aggregate and fiber reinforcement respectively; (2) uniformly mixing the modified recycled coarse aggregate, fine aggregate, cement and water reducing agent to obtain a mixed material; (3) Mix water and fiber reinforcement with the mixed material to obtain concrete mortar; pour the mortar into a mold, demould after molding, and obtain high-strength concrete after curing.

Citation Information

Patent Citations

  • Preparation method of titanium-dioxide-modified carbon-fiber-reinforced resin-base composite material

    CN105602000A

  • Modified coarse aggregate, fiber nano recycled concrete prepared from modified coarse aggregate and preparation method of fiber nano recycled concrete

    CN110105018A

  • High-durability maritime work concrete doped with modified silica sol and preparation method of high-durability maritime work concrete

    CN114890751A

  • Method for preparing high-strength concrete from construction waste recycled aggregate

    CN115403323A

  • Self-compacting durable concrete and preparation method thereof

    CN116768548A

Cited By

  • Fiber reinforced concrete based on building solid waste recycled aggregate and preparation method thereof

    CN120463454A