Modified biomass firework cylinder material and preparation method thereof

Through the preparation method of modified biomass fireworkscope materials, combined with polyvinylamide, modifier and admixture, the problems of mold release and adhesion during the molding of biomass material are solved, and high mechanical strength and low cost are achieved Forming materials have promoted the large-scale production and marketing promotion of biomass materials.

CN118930208APending Publication Date: 2024-11-12QINGDAO HUOLINHE NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410998878.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the molding process, existing biomass materials are prone to dismantling and rebound problems, which makes it difficult to achieve large-scale production and marketing promotion. The traditional fireworks sysfunction materials are costly and cannot effectively utilize farmland straw and other recycling. Utilize resources.

Method used

Modified biomass fireworks and its preparation method are adopted, and the production line of injection molding-release-stacking-curing is adopted to avoid mold release and adhesions by reasonably proportioning biomass materials with polyvinylamide, modifiers and admixtures. The problem of rebound and the use of cement, gypsum powder and other components to improve the mechanical strength and toughness of the material.

Benefits of technology

It realizes high mechanical strength, toughness and low cost of biomass materials, solves the problems of mold release adhesion and rebound, reduces production costs, improves production efficiency, is easy to promote to the market, and the materials are easy to store and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a modified biomass firework cylinder material and a preparation method thereof. The modified biomass firework cylinder material comprises the following components in parts by weight: 10-90 parts of a biomass material; 0.1 to 0.3 part of polyethylene amide; a modifier: 0.2 to 0.4 part of a biomass mildew preventive, 0.1 to 0.2 part of methyl cellulose, 0.01 to 0.3 part of plant phospholipase, and 0.5 to 10 parts of a modified emulsion; the additive is one or more of cement, gypsum powder, fine sand, lightweight aggregate, a water reducing agent, waterproof rubber powder, a waterproof agent, pregelatinized starch, pp fibers, a thickening agent and a lubricating agent. According to the modified biomass firework cylinder material and the preparation method thereof, the raw materials are easy to obtain, the manufacturing cost is low, a modification-mixing-injection molding-demolding-stacking-curing production line is formed, the problems of demolding adhesion and rebound after demolding are avoided, firework bases, firework cylinders, product packaging materials and other forming materials can be prepared, and the production cost is low. The material has the advantages of high mechanical strength, good toughness, low cost, easy storage, easy popularization and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new materials, and in particular to a modified biomass firework tube material and a preparation method thereof. Background Art

[0002] Every summer harvest and autumn and winter, a large amount of wheat, corn and other straw is often burned in the fields, producing a lot of thick smoke, which has not only become a bottleneck problem for rural environmental protection, but also a culprit for the harm to the urban environment, and also wastes a lot of recyclable resources. According to relevant statistics, my country can generate more than 1 billion tons of straw every year, which has become "waste" that is "not very useful" but must be disposed of. In this case, if it is completely handled by farmers, a large amount of straw will be burned and buried in farmland, which has no value for recycling.

[0003] my country is the main producer of fireworks. The use of fireworks is becoming more and more popular in my country and even overseas, and the consumption is very large. Traditional fireworks outer tubes are mainly made by hand and hot pressing, and the main raw materials are paper and waste paper pulp. Straw and other biomass materials have not been used in the field of fireworks. Making them into fireworks bases and fireworks tubes will consume a lot of farmland straw, which can solve the problem of farmers dealing with straw.

[0004] In the prior art, since biomass materials have good toughness and expansion force, there are often still gaps inside them after compaction, and it is even difficult for the board to solidify, cannot be immediately separated from the mold, sticks to the mold, and rebounds after demolding. The only way is to reduce the proportion of biomass materials and occupy a large number of molds for a long time, making it difficult to achieve large-scale production capacity and put it into practical use in the market.

[0005] Therefore, the modification of biomass materials is very important. Only by removing its expansion force and reducing sugar content and reasonable proportion can it be used in molding materials to better play its advantages of light weight and low cost. Therefore, a preparation method of modified biomass firework base and firework tube material is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a modified biomass firework tube material and a preparation method thereof. The raw materials are easily available and low in cost. A production line of modification-mixing-injection molding-demolding-stacking-curing is formed to avoid the problems of demolding adhesion and rebound after demolding. The material can be made into firework bases, firework tubes, product packaging materials and other molding materials, and has the advantages of high mechanical strength, good toughness, low cost, easy storage and easy promotion.

[0007] To achieve the above object, the present invention provides a modified biomass firework tube material, comprising the following components in parts by weight:

[0008] 10-90 parts of biomass materials;

[0009] Polyvinyl amide 0.1-0.3 parts;

[0010] Modifier: 0.1-0.4 parts of biomass mildew inhibitor, 0.1-0.2 parts of methyl cellulose, 0.01-0.3 parts of plant phospholipase, 0.5-10 parts of modified latex;

[0011] The admixture is one or more of cement, gypsum powder, fine sand, lightweight aggregate, water reducing agent, waterproof rubber powder, waterproofing agent, pregelatinized starch, PP fiber, thickener and lubricant.

[0012] Preferably, the biomass material is one or more of farm straw, sawdust, bagasse, bark, hay, grain bran and wood powder.

[0013] Preferably, the weight percentage of the admixture is as follows:

[0014] 5-15 parts of cement, 10-80 parts of gypsum powder, 5-15 parts of fine sand, 0.5-20 parts of lightweight aggregate, 0.1-0.3 parts of water reducing agent, 0.1-0.5 parts of waterproof glue powder, 0.1-0.5 parts of waterproofing agent, 0.1-0.5 parts of thickener, 0.1-0.5 parts of pregelatinized starch, 0.1-0.5 parts of pp fiber, and 0.1-0.3 parts of lubricant.

[0015] Preferably, the cement is ordinary Portland cement;

[0016] The gypsum powder is one or more of natural gypsum powder, desulfurized gypsum powder, phosphogypsum powder and dihydrate gypsum powder;

[0017] The lightweight aggregate is one or more of vitrified microspheres, perlite, vermiculite, slag, and ceramsite.

[0018] To achieve the above object, the present invention also provides a method for preparing a modified biomass firework tube material, comprising the following steps:

[0019] S1. Cut and crush the biomass material with a moisture content of less than 5-10% to obtain a biomass material with a length of 1-20 mm;

[0020] S2. Adding a modifier and water to the biomass material by weight, stirring and mixing to form a paste-like mixture, thereby obtaining a modified biomass material;

[0021] S3, injecting an admixture into the modified biomass material obtained in the above step S2, stirring and mixing, and obtaining a granular or paste-like mixture;

[0022] S4, adding polyacrylamide to the granules or paste mixture obtained in the above step S3, stirring evenly, putting the cloth into a mold, extruding or stamping by special molding equipment, demolding, and stacking for curing;

[0023] S5. After curing, the film is packaged and ready for shipment.

[0024] Preferably, in step S2, the stirring time is 3 minutes.

[0025] Preferably, in step S3, the stirring time is 5 min, and the speed of the stirring paddle is 60 r / min.

[0026] Preferably, in step S4, the stirring time is 2 min, the speed of the stirring paddle is 60 r / min, and the speed of the stirring paddle is 60 r / min.

[0027] Preferably, in step S4, the extrusion or stamping molding using special molding equipment is specifically: extrusion molding is performed using hot extrusion, cold extrusion or cold stamping equipment, the curing time after hot extrusion molding is 1 hour, and the curing time after cold extrusion or cold stamping molding is 10-28 days.

[0028] Therefore, the present invention adopts the above-mentioned modified biomass firework tube material and preparation method thereof, and the beneficial effects are as follows:

[0029] (1) Compared with the prior art, the cost of pulp or waste pulp is relatively high, and the admixture composition and process cannot realize cold pressing molding technology. The raw materials used in the present invention are easy to obtain and low in cost. After being mixed in a reasonable proportion, they form a production line and enter the assembly line of modification-mixing-injection molding-demolding-stacking-curing. It is completed in one go, has high production efficiency, and is easy to promote to the market to achieve large-scale production capacity.

[0030] (2) The present invention first modifies the biomass material so that the biomass material retains crude fiber but loses elasticity and reduces sugar content, and then mixes it with cement and gypsum powder to avoid the problems of demolding adhesion and rebound after demolding. The resulting molding material is light in weight, has high mechanical strength, toughness and stable performance.

[0031] (3) The present invention adds biological mildew inhibitors and waterproofing agents, which will not affect the durability of the finished material due to the high specific gravity of the biomass material, and play a role in anti-corrosion and easy storage. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further illustrated by the following examples.

[0033] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0034] Embodiment 1

[0035] A modified biomass firework tube material using a cold extrusion molding device comprises the following components in parts by weight:

[0036] 15 parts of biomass materials;

[0037] Polyvinyl amide 0.2 parts;

[0038] Modifier: 0.2 parts of biomass mildew inhibitor, 0.1 parts of methyl cellulose, 0.04 parts of plant phospholipase, and 0.7 parts of modified latex;

[0039] Admixtures: 5 parts of cement, 75 parts of gypsum powder, 5 parts of fine sand, 0.2 parts of waterproof glue powder, 0.2 parts of water reducing agent, 0.2 parts of PP fiber, and 0.3 parts of waterproofing agent.

[0040] The preparation method is as follows:

[0041] S1. Cut and crush farmland straw with a moisture content of less than 5-10% to obtain farmland straw with a length of 1-20 mm, and put it into a stirring tank with a stirring paddle rotating at 60 r / min;

[0042] S2. Add the modifier and water in parts by weight into a stirring tank and stir for 3 minutes until completely mixed to form a paste-like mixture to obtain a modified biomass material;

[0043] S3, injecting the additive into the modified biomass material obtained in the above step S2, stirring for 5 minutes until completely mixed, to obtain a granular or paste-like mixture;

[0044] S4, adding polyvinyl amide to the granules or paste mixture obtained in the above step S3, stirring for 2 minutes until the mixture is uniform, and then putting it into a mold, using a special cold extrusion equipment to extrude for 5 seconds, demolding, and stacking for curing for 18 days to obtain a uniform and densely pressed mixture product;

[0045] S5. After curing, the finished products are packed with film and stacked neatly for shipment.

[0046] Embodiment 2

[0047] A modified biomass firework tube material using a cold stamping forming device comprises the following components in parts by weight:

[0048] 15 parts of biomass materials;

[0049] Polyvinyl amide 0.1 part;

[0050] Modifier: 0.3 parts of biomass mildew inhibitor, 0.1 parts of methyl cellulose, 0.04 parts of plant phospholipase, and 0.7 parts of modified latex;

[0051] Admixtures: 75 parts of gypsum powder, 0.5 parts of lightweight aggregate, 5 parts of cement, 5 parts of fine sand, 0.3 parts of waterproof glue powder, and 0.1 parts of lubricant.

[0052] The preparation method is as follows:

[0053] S1. Cut and crush farmland straw with a moisture content of less than 5-10% to obtain farmland straw with a length of 1-20 mm, and put it into a stirring tank with a stirring paddle rotating at 60 r / min;

[0054] S2. Add the modifier and water in parts by weight into a stirring tank and stir for 3 minutes until completely mixed to form a paste-like mixture to obtain a modified biomass material;

[0055] S3, injecting the additive into the modified biomass material obtained in the above step S2, stirring for 5 minutes until completely mixed, to obtain a granular or paste-like mixture;

[0056] S4, adding polyvinyl amide to the granules or paste mixture obtained in the above step S3, stirring for 2 minutes until the mixture is uniform, and then putting it into a mold, using special cold stamping equipment for stamping, demolding, and stacking for curing for 18 days to obtain a uniform and densely pressed mixture product;

[0057] S5. After curing, the finished products are packed with film and stacked neatly for shipment.

[0058] Embodiment 3

[0059] A modified biomass firework tube material using a hot extrusion molding device comprises the following components in parts by weight:

[0060] 20 parts of biomass materials;

[0061] Polyvinyl amide 0.2 parts;

[0062] Modifier: 0.3 parts of biomass mildew inhibitor, 0.1 parts of methyl cellulose, 0.03 parts of plant phospholipase, 0.7 parts of modified latex;

[0063] Admixtures: 80 parts of gypsum powder, 0.3 parts of thickener, 0.5 parts of waterproof rubber powder, 0.1 parts of lubricant, 0.3 parts of waterproof agent, and 0.2 parts of PP fiber.

[0064] The preparation method is as follows:

[0065] S1. Cut and crush farmland straw with a moisture content of less than 5-10% to obtain farmland straw with a length of 1-20 mm, and put it into a stirring tank with a stirring paddle rotating at 60 r / min;

[0066] S2. Add the modifier and water in parts by weight into a stirring tank and stir for 3 minutes until completely mixed to form a paste-like mixture to obtain a modified biomass material;

[0067] S3, injecting the additive into the modified biomass material obtained in the above step S2, stirring for 5 minutes until completely mixed, to obtain a granular or paste-like mixture;

[0068] S4, adding polyvinyl amide to the granules or paste mixture obtained in the above step S3, stirring for 2 minutes until the mixture is uniform, and then putting it into a mold, using a special hot extrusion molding equipment to extrude for 3-6 minutes, demolding, and stacking for curing for 1 hour to obtain a uniform and densely pressed mixed product;

[0069] S5. After curing, the finished products are packed with film and stacked neatly for shipment.

[0070] Embodiment 4

[0071] The difference from the third embodiment is that a modified biomass firework tube material using a hot extrusion molding device comprises the following components in parts by weight:

[0072] 60 parts of biomass materials;

[0073] Polyvinyl amide 0.2 parts;

[0074] Modifier: 0.2 parts of biomass mildew inhibitor, 0.1 parts of methyl cellulose, 0.05 parts of plant phospholipase, 0.7 parts of modified latex;

[0075] Admixtures: 40 parts of gypsum powder, 0.3 parts of waterproof rubber powder, 0.1 parts of thickener, 0.5 parts of pregelatinized starch, 0.1 parts of lubricant, 0.3 parts of waterproof agent, and 0.3 parts of PP fiber.

[0076] Embodiment 5

[0077] The difference from the third embodiment is that a modified biomass firework tube material using a hot extrusion molding device comprises the following components in parts by weight:

[0078] 80 parts of biomass materials;

[0079] Polyvinyl amide 0.2 parts;

[0080] Modifier: 0.3 parts of biomass mildew inhibitor, 0.1 parts of methyl cellulose, 0.05 parts of plant phospholipase, and 0.8 parts of modified latex;

[0081] Admixtures: 20 parts of gypsum powder, 0.6 parts of waterproof rubber powder, 0.2 parts of lubricant, 0.5 parts of waterproof agent, 0.3 parts of thickener, 0.5 parts of pregelatinized starch, and 0.3 parts of PP fiber.

[0082] Experimental Testing

[0083] The molding materials prepared in Examples 1 to 5 were used to assemble a firework base with a size of 190 mm × 190 mm × 240 mm-25 holes. The toughness and mechanical strength of the firework base were described by the flexural strength and compressive strength tests, which were measured using a flexural and compressive testing machine. The weight of the firework base was measured multiple times using an industrial weight scale, and the average value was taken. The specific test results were statistically shown in Table 1.

[0084] Table 1 Average weight and mechanical strength test statistics

[0085]

[0086] Therefore, the present invention adopts the above-mentioned modified biomass firework tube material and its preparation method, the raw materials are easy to obtain and the cost is low, and a modification-mixing-injection molding-demolding-stacking-curing production line is formed to avoid the problems of demolding adhesion and rebound after demolding. It can be made into molding materials such as firework bases, firework tubes and product packaging materials, and has the advantages of high mechanical strength, good toughness, low cost, easy storage and easy promotion.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A modified biomass firework tube material, characterized in that: The composition comprises the following components by weight: 10-90 parts of biomass materials; Polyvinyl amide 0.1-0.3 parts; Modifier: 0.1-0.4 parts of biomass mildew inhibitor, 0.1-0.2 parts of methyl cellulose, 0.01-0.3 parts of plant phospholipase, 0.5-10 parts of modified latex; The admixture is one or more of cement, gypsum powder, fine sand, lightweight aggregate, water reducing agent, waterproof rubber powder, waterproofing agent, pregelatinized starch, PP fiber, thickener and lubricant.

2. A modified biomass firework tube material according to claim 1, characterized in that: The biomass material is one or more of farmland straw, sawdust, bagasse, bark, hay, grain bran and wood powder.

3. The modified biomass firework tube material according to claim 1, characterized in that: The weight parts of the admixture are specifically as follows: 5-15 parts of cement, 10-80 parts of gypsum powder, 5-15 parts of fine sand, 0.5-20 parts of lightweight aggregate, 0.1-0.3 parts of water reducing agent, 0.1-0.5 parts of waterproof glue powder, 0.1-0.5 parts of waterproofing agent, 0.1-0.5 parts of thickener, 0.1-0.5 parts of pregelatinized starch, 0.1-0.5 parts of pp fiber, and 0.1-0.3 parts of lubricant.

4. The modified biomass firework tube material according to claim 3, characterized in that: The cement is ordinary Portland cement; The gypsum powder is one or more of natural gypsum powder, desulfurized gypsum powder, phosphogypsum powder and dihydrate gypsum powder; The lightweight aggregate is one or more of vitrified microspheres, perlite, vermiculite, slag, and ceramsite.

5. A method for preparing the modified biomass firework tube material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Cut and crush the biomass material with a moisture content of less than 5-10% to obtain a biomass material with a length of 1-20 mm; S2. Adding a modifier and water to the biomass material by weight, stirring and mixing to form a paste-like mixture, thereby obtaining a modified biomass material; S3, injecting an admixture into the modified biomass material obtained in the above step S2, stirring and mixing, and obtaining a granular or paste-like mixture; S4, adding polyacrylamide to the granules or paste mixture obtained in the above step S3, stirring evenly, putting the cloth into a mold, extruding or stamping by special molding equipment, demolding, and stacking for curing; S5. After curing, the film is packaged and ready for shipment.

6. The method for preparing a modified biomass firework tube material according to claim 5, characterized in that: In step S2, the stirring time is 3 minutes.

7. The modified biomass firework tube material and preparation method thereof according to claim 5, characterized in that: In step S3, the stirring time is 5 minutes, and the speed of the stirring paddle is 60 r / min.

8. The method for preparing a modified biomass firework tube material according to claim 5, characterized in that: In step S4, the stirring time is 2 min, the speed of the stirring paddle is 60 r / min, and the speed of the stirring paddle is 60 r / min.

9. The method for preparing a modified biomass firework tube material according to claim 5, characterized in that: In step S4, the extrusion or stamping is performed using special molding equipment, specifically: hot extrusion, cold extrusion or cold stamping equipment is used for extrusion molding, the curing time after hot extrusion molding is 1 hour, and the curing time after cold extrusion or cold stamping molding is 10-28 days.