ZnBiMnGeO-based voltage-sensitive ceramic material and preparation method thereof
By using GeO2 doping in ZnO-based pressure-sensitive ceramics and using low-temperature sintering technology to form eutectic liquid phase and strengthen the grain boundary, the problems of energy consumption and leakage current of high-temperature sintering of ZnO-based pressure-sensitive ceramics are solved, and low-cost High-performance varistor ceramic materials with low leakage current have promoted the green development of the varistor industry.
Patent Information
- Application Number
- CN202411066278.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
The existing ZnO-based pressure-sensitive ceramic materials consume a lot of energy during high-temperature sintering, with high costs and large leakage current, which hinders the industry's energy conservation, consumption reduction and green production.
GeO2 is used as the main dopant, and ZnBiMnGeO ceramics are sintered at low temperature through traditional solid phase technology to form eutectic liquid phase, reduce the sintering temperature, and strengthen the grain boundary barrier through Ge doping to optimize the performance of the ceramic.
Low-temperature sintering is achieved, reducing production costs, reducing leakage current density, and providing green and sustainable pressure-sensitive ceramic materials suitable for resistance applications in high and low voltage fields.
Smart Images

Figure CN118930245A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic preparation, and in particular to a ZnBiMnGeO-based varistor ceramic material and a preparation method thereof. Background Art
[0002] ZnO-based varistor is a nonlinear resistor material whose internal resistance can change repeatedly with the height of the applied voltage relative to a certain critical voltage (the so-called varistor voltage). When the applied voltage is lower than the varistor voltage, the internal electrode of the ZnO-based varistor is very large, similar to an insulating body; when the high applied voltage is higher than the varistor voltage, its internal resistance will be reduced to a conductor state in an instant. Based on this characteristic, ZnO-based varistors made of ZnO varistor ceramics are often connected to the circuit in parallel with the protected circuit or device to prevent abnormal surge voltage from damaging the protected circuit or device. At present, the application range of ZnO-based varistors has covered almost all electronic and electrical fields such as low voltage, medium voltage and high voltage, becoming the world's largest abnormal voltage surge protection device.
[0003] All ZnO-based varistor ceramics use ZnO powder as the main raw material. On this basis, common high-performance ZnO-based varistor ceramics need to further add Bi 2 O 3 、V 2 O 5 , Pr 2 O 3 (Pr 6 O 11 ),Cr 2 O 3 , Sb 2 O 3 、MnO 2 、Co 2 O 3 , Nb 2 O 5 , CaO, and various rare earth oxides, etc., which ultimately leads to the fact that most high-performance ZnO-based varistors often have as many as 6 or even more components. This multi-component ZnO-based varistors will undoubtedly increase the impact of the entire varistor industry on the increasingly scarce natural resources.
[0004] Regardless of the preparation process, the ZnO powder and various dopings must undergo a high-temperature sintering process to become varistors. The sintering temperature of most high-performance ZnO-based varistors is higher than 1000°C, and some are even higher, reaching above 1200°C. In order to meet such a high sintering temperature, electronic device factories that produce varistors not only need more expensive high-temperature sintering equipment, but these equipment will also inevitably consume more electricity during the production process. In the process of producing low-voltage chip varistors using the stacking co-firing process, the internal electrode must use alloys with high precious metal content such as Pt or Pd, and cannot use low-melting-point base metals such as Cu (melting point 1083°C), which are more expensive. These factors are the main reasons that hinder the entire ZnO-based varistors industry from saving energy and reducing consumption and achieving green production.
[0005] In addition, when ZnO-based varistors are used in actual electronic circuits as abnormal voltage surge protection devices, even if the external field voltage it bears is less than its varistor voltage, a certain current will pass through it. This current is the so-called leakage current, referred to as leakage current, and its magnitude is expressed by leakage current density. Therefore, leakage current becomes the main cause of reactive power loss of ZnO-based varistors in practical applications. In order to reduce the reactive power loss of ZnO-based varistors in practical applications, it is necessary to use ZnO-based varistor ceramics with as low leakage current as possible. Summary of the invention
[0006] In view of the existing problems, the present invention provides a GeO 2 ZnBiMnGeO varistor ceramic material as main doping modification material and preparation method thereof.
[0007] The technical solution of the present invention:
[0008] A ZnBiMnGeO simple component varistor ceramic, under the condition that the total molar content of the four elements Zn, Bi, Mn and Ge is 100%, the molar percentages of the three elements Bi, Mn and Ge are respectively: Bi is 0.5-5%, Mn is 1-4%, and Ge is 0.05-0.5%.
[0009] The raw materials are oxides of four metal elements, Zn, Bi, Mn and Ge, or compounds such as carbonates, nitrates, acetates or hydroxides that can be decomposed into the above metal oxides, or pre-synthesized products using the oxides or other compounds of the above four elements as raw materials, such as Bi 2 O 3 With Mn 2 O 3 or GeO 2 Bi synthesized by preheating reaction 2 O 3 ·2Mn 2 O 3or 6Bi 2 O 3 ·GeO 2 type oxide solid solution.
[0010] The method for preparing the ZnBiMnGeO-based varistor ceramic material comprises the following steps:
[0011] (1) According to the molar ratio of Zn, Bi, Mn and Ge in the varistor ceramic material, ZnO, Bi 2 O 3 、MnCO 3 and GeO 2 Raw materials, and then the ceramic green body is prepared by conventional solid phase process;
[0012] (2) Sintering the debinding green body to 875-1000° C. at a heating rate of 2-15° C. / min and keeping the temperature for 1-6 hours. Finally, cooling the green body to room temperature naturally in the furnace to obtain a varistor ceramic material.
[0013] Preferably, the green body after debinding is heated to 975° C. at a heating rate of 4° C. / min, sintered, and kept at this temperature for 3 hours.
[0014] The varistor ceramic can also adopt the existing tape-casting ceramic synthesis process.
[0015] Beneficial effects of the present invention:
[0016] (1) The varistor ceramic material of the present invention has ZnO as the main component, wherein the ZnO content is above 90%, and only three doping components, Bi, Mn and Ge, are added to ZnO to obtain a ZnBiMnGeO-based varistor ceramic material.
[0017] (2) The present invention adopts the traditional solid phase synthesis process, and the GeO 2 with Bi 2 O 3 The eutectic liquid phase can begin to form at about 882°C, which increases the amount of liquid phase generated during the sintering process and allows the ceramic to be sintered at a low temperature of 975°C. The sintering temperature (975°C) is significantly lower than the melting point of Cu, 1083°C. The low-temperature sintering feature can not only reduce the sintering cost during the preparation of the monomeric ZnO-based varistor, but also allow manufacturers to use the ZnBiMnGeO-based varistor ceramic of the present invention as a raw material, and use base metals such as Cu to replace Pt or Ag-Pd alloys with higher melting points and prices as internal electrodes to prepare low-voltage chip-type laminated ZnO-based varistors.
[0018] (3) The cooling after sintering of the present invention adopts a natural cooling method. The slow cooling can not only release the stress on the internal grain boundaries of the ZnO-based varistor ceramic, but also allow the doped ions dissolved in the ZnO grains and the above-mentioned eutectic liquid phase at high temperature to have a longer time to dissolve to the ZnO grain boundaries, so that the obtained ZnO-based ceramic has better varistor properties.
[0019] (4) The present invention strengthens the grain boundary barrier by doping Ge on the ZnO grain boundary to form donor doping and zinc vacancy defects, thereby optimizing the performance of the ZnBiMnGeO varistor ceramic;
[0020] (5) The ZnBiMnGeO varistor ceramic of the present invention has excellent electrical properties, with a varistor voltage of 120 to 340 V / mm, a nonlinear coefficient α greater than 40, and a leakage current density J L <10μA / cm 2 .
[0021] (6) In the current situation of increasingly scarce natural resources and energy, the present invention provides a ZnO-based varistor material that simultaneously meets the requirements of simplified components, low sintering temperature, and low leakage current, providing a new idea for the green and sustainable development of the entire varistor industry.
[0022] (7) The novel varistor ceramic material of the present invention is not only suitable for bulk ZnO-based varistors in the high and medium voltage fields, but also for chip-type laminated ZnO-based varistors in the low voltage application field. It is an ideal substitute for various ZnO varistor ceramic materials with a sintering temperature higher than 1000°C. The related products can be used as high-voltage power transmission and lightning arresters, overvoltage protectors for medium-voltage vehicles, and overvoltage protectors for integrated circuits in the low voltage field, etc., and have a very broad market prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is the EJ curve of the ZnBiMnGeO varistor ceramic involved in Example 1;
[0024] Figure 2 is the EJ curve of the ZnBiMnGeO varistor ceramic involved in Example 2;
[0025] Figure 3 This is the EJ curve of the ZnBiMnGeO varistor ceramic involved in Example 3. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0027] Table 1 Ceramic powder formulations of various embodiments (mol%)
[0028] raw material ZnO <![CDATA[Bi 2 THE 3 ]]> <![CDATA[MnCO 3 ]]> <![CDATA[GeO 2 ]]> Example 1 97.44 0.50 2.00 0.06 Example 2 97.40 0.50 2.00 0.10 Example 3 97.35 0.50 2.00 0.15
[0029] Embodiment 1: A method for preparing a ZnBiMnGeO-based high-performance varistor ceramic material, comprising the following steps:
[0030] (1) According to the formula of ceramic powder, the molar percentages of each raw material are: ZnO 97.44, Bi 2 O 3 0.5, MnCO 3 2 and GeO 2 0.06;
[0031] The ceramic green body was prepared by a conventional solid phase process, and the specific process was as follows: a planetary ball mill was used, and zirconium oxide balls and anhydrous ethanol were used as ball milling media to ball mill all the raw materials for 12 hours; the ball-milled raw material slurry was placed in an oven at 80°C and dried for 24 hours; the dried raw materials were mixed with an appropriate amount of polyvinyl alcohol with a concentration of 5%, and after granulation, they were compressed into a green body with a diameter of 12 mm and a thickness of about 1.2 mm; the green body was heated to 500°C at a heating rate of 1°C / min, and kept warm for 1 hour to perform debinding (i.e., expel the polyvinyl alcohol);
[0032] (2) The debinding green body is sintered to 975°C at a heating rate of 4°C / min and kept at this temperature for 3 hours. Finally, the green body is naturally cooled to room temperature in the furnace to obtain the zinc oxide-based varistor ceramic sample of the present invention.
[0033] The upper and lower surfaces of the sintered sample were polished to make silver electrodes, and their EJ curves were measured. Figure 1 shown. Figure 1 It shows that the nonlinear transition of the EJ curve of the sample from the low current density area to the high current density area presents a "knee-shaped" change trend that a typical varistor should have; and the "knee-shaped area" is close to a right angle, indicating that the sample has good nonlinear electrical properties. On this basis, the nonlinear coefficient α and the varistor voltage E of the tested sample are calculated respectively. b , leakage current density J L , the results are shown in Table 2.
[0034] Table 2 Performance indicators of varistor ceramics of Example 1
[0035]
[0036] Table 2 shows that the nonlinear coefficient α of the product in Example 1 is as high as 48.62, the varistor voltage is 338.10V / mm, and the average grain diameter is 7.47μm; at the same time, its leakage current density is only 6.09μA / cm 2 .
[0037] Embodiment 2: A method for preparing a ZnBiMnGeO-based varistor ceramic material, comprising the following steps:
[0038] (1) According to the formula of ceramic powder, the molar percentages of each raw material are: ZnO 97.40, Bi 2 O 3 0.5, MnCO 3 2 and GeO 2 0.1;
[0039] The ceramic green body was prepared by a conventional solid phase process. Specifically, a planetary ball mill was used to mill all the raw materials for 12 hours using zirconium oxide balls and anhydrous ethanol as the ball milling medium; the raw material slurry after ball milling was placed in an oven at 80°C for drying for 24 hours; the dried raw material was mixed with an appropriate amount of polyvinyl alcohol with a concentration of 5%, and the green body was compressed into a green body with a diameter of 12 mm and a thickness of about 1.2 mm after granulation; the green body was heated to 500°C at a heating rate of 1°C / min, kept warm for 1 hour, and debinding (i.e., debinding the polyvinyl alcohol);
[0040] (2) Sintering the debinding green body to 975°C at a heating rate of 4°C / min and keeping the temperature for 3 hours, and finally cooling the green body to room temperature naturally in the furnace to obtain a zinc oxide-based varistor ceramic.
[0041] The upper and lower surfaces of the sintered sample were polished to make silver electrodes, and their EJ curves were measured. Figure 2 shown. Figure 2 It shows that the nonlinear transition of the EJ curve of the sample from the low current density area to the high current density area also shows the "knee-shaped" change trend that a typical varistor should have; and the "knee-shaped area" is close to a right angle, indicating that the sample has good nonlinear electrical properties. On this basis, the nonlinear coefficient α and the varistor voltage E of the tested sample are calculated respectively. b , leakage current density J L ,The results are summarized in Table 3.
[0042] Table 3 Performance indicators of varistor ceramics of Example 2
[0043]
[0044] The data in Table 3 show that as GeO 2 With the increase of doping amount, the average grain size increases to 7.63μm, and the varistor voltage drops to 201.61V / mm; the nonlinear coefficient decreases slightly, but is still greater than 40; the leakage current density is 7.28μA / cm 2 Lower level.
[0045] Embodiment 3: A method for preparing a ZnBiMnGeO-based varistor ceramic material, comprising the following steps:
[0046] (1) According to the formula of ceramic powder, the molar percentages of each raw material are: ZnO 97.35, Bi 2 O 3 0.5, MnCO 3 2 and GeO 2 0.15;
[0047] The ceramic green body was prepared by a conventional solid phase process, and the specific process was as follows: a planetary ball mill was used, and zirconium oxide balls and anhydrous ethanol were used as ball milling media to ball mill all the raw materials for 12 hours; the ball-milled raw material slurry was placed in an oven at 80°C and dried for 24 hours; the dried raw materials were mixed with an appropriate amount of polyvinyl alcohol with a concentration of 5%, and after granulation, they were compressed into a green body with a diameter of 12 mm and a thickness of about 1.2 mm; the green body was heated to 500°C at a heating rate of 1°C / min, and kept warm for 1 hour to perform debinding (i.e., expel the polyvinyl alcohol);
[0048] (2) Sintering the debinding green body to 975°C at a heating rate of 4°C / min and keeping the temperature for 3 hours, and finally cooling the green body to room temperature naturally in the furnace to obtain a zinc oxide-based varistor ceramic.
[0049] The upper and lower surfaces of the sintered sample were polished to make silver electrodes, and their EJ curves were measured. Figure 3 shown. Figure 3 It shows that the nonlinear transition of the EJ curve of the sample from the low current density area to the high current density area also shows the "knee-shaped" change trend that a typical varistor should have; and the "knee-shaped area" is close to a right angle, indicating that the sample has good nonlinear electrical properties. On this basis, the nonlinear coefficient α and the varistor voltage E of the tested sample are calculated respectively. b , leakage current density J L ,The results are summarized in Table 4.
[0050] Table 4 Performance indicators of varistor ceramics of Example 3
[0051]
[0052] Table 4 shows that with the increase of GeO2 doping amount, the average grain size increases to 7.80μm, and the varistor voltage decreases to 129.24V / mm. The nonlinear coefficient α can still be maintained at a high level above 40. The leakage current density is only 8.55μA / cm2.
[0053] The ZnO-based varistor ceramic of the present invention is prepared by solid phase sintering process and can be completely sintered at a low temperature of 975°C. High-performance varistor ceramics with a nonlinear coefficient of more than 40, a varistor voltage of 100 to 400 V / mm, and a leakage current density of less than 10 μA / cm2 can be prepared by adding only a very small amount of GeO2 (0.05 to 0.5%, molar percentage).
[0054] The sintering temperature (975°C) of the process of the present invention is significantly lower than the melting point of Cu, 1083°C. This low-temperature sintering feature can not only reduce the sintering cost in the preparation process of ZnO-based varistors, but also allow manufacturers to use the ZnBiMnGeO-based varistor of the present invention as a raw material, and use base metals such as Cu to replace Pt or Ag-Pd alloys with higher melting points and prices as internal electrodes to prepare low-voltage chip-type laminated ZnO-based varistors. In short, the high-performance ZnBiMnGeO varistor of the present invention provides a new idea for the low-cost green production and application of ZnO-based varistors.
Claims
1. A ZnBiMnGeO-based varistor ceramic material, characterized in that: The material is composed of five elements: O, Zn, Bi, Mn and Ge. Under the condition that the total molar content of the four elements is 100%, the molar percentages of the three elements Bi, Mn and Ge are respectively: 0.5-5%, 1-4%, 0.05-0.5%, and the rest is Zn element.
2. The ZnBiMnGeO-based varistor ceramic material according to claim 1, characterized in that: The raw materials of the varistor ceramic material are oxides, carbonates, nitrates, acetates or hydroxides of four metal elements: Zn, Bi, Mn and Ge.
3. A method for preparing the ZnBiMnGeO-based varistor ceramic material according to claim 1, characterized in that: According to the molar ratio of the four elements Zn, Bi, Mn and Ge in the varistor ceramic material, ZnO, Bi2O3, MnCO3 and GeO2 are weighed, and then a ceramic green body is prepared by a conventional solid phase process; The debinding green body is sintered to 875-1000°C at a heating rate of 2-15°C / min, and kept at the temperature for 1-6 hours. Finally, the green body is naturally cooled to room temperature in the furnace to obtain a varistor ceramic material.
4. The method for preparing the ZnBiMnGeO-based varistor ceramic material according to claim 3, characterized in that: The method for preparing a ceramic green body by the traditional solid phase process is as follows: after mixing the raw materials, adding them into a planetary ball mill and ball milling them for 12 hours to obtain a powder; placing the powder into an oven at 80°C and drying it for 24 hours, mixing the powder with an appropriate amount of polyvinyl alcohol, granulating it, and compressing it into a green body with a diameter of 12 mm; heating the green body to 500°C at a heating rate of 1°C / min, keeping it warm for 1 hour, and debinding it.
5. The method for preparing the ZnBiMnGeO-based varistor ceramic material according to claim 3, characterized in that: The green body after debinding was heated to 975°C at a heating rate of 4°C / min, sintered, and kept at this temperature for 3 hours.
Citation Information
Patent Citations
Voltage nonlinear resistor
JP1999031605A