Silver niobate energy storage ceramic with efficient grain size effect and preparation method of silver niobate energy storage ceramic
The preparation of silver niobate ceramics through solid phase reaction method and SPS sintering technology solved the problems of insufficient grain size effect and unstable preparation in the prior art, achieved efficient energy storage performance improvement and cost reduction, and significantly improved niobate acid The energy storage density of silver ceramics.
Patent Information
- Application Number
- CN202410903158.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to effectively prepare silver niobate ceramics with obvious grain size effects, resulting in low energy storage performance, unstable preparation process and high cost.
Single-phase AN pre-fired powder was prepared by solid phase reaction method, and a dense ceramic body with obvious grain size effect was obtained by SPS sintering technology at lower temperatures. Pressure was applied in real time to increase density, and through decarbonization treatment and Electrode sintering further optimizes the structure.
The energy storage performance of silver niobate is significantly improved. Compared with ceramics without grain size effect, its energy storage performance can be improved by up to 92%, and the sintering temperature is reduced, achieving dense structural structure and fine grains of the ceramic body.
Smart Images

Figure CN118930262A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silver niobate ceramic material, in particular to a silver niobate energy storage ceramic with high-efficiency grain size effect and a preparation method thereof, belonging to the technical field of dielectric energy storage ceramics. Background Art
[0002] Dielectric energy storage capacitors have fast charge and discharge rates (~ns) and high power density (~10 8 W / kg) and long cycle life (~50,000 times), and are widely used in new energy power generation systems, hybrid vehicles, medical devices, spacecraft, satellites, and pulse weapon systems. However, the low energy density is the main reason that limits its use in terminal products with miniaturization and integration development needs. As an important lead-free antiferroelectric material, AgNbO3 has high saturation polarization, low remnant polarization, and high energy density, but its effective energy density is relatively low compared with traditional lead-based antiferroelectric materials.
[0003] Since the grain size has a significant effect on the breakdown electric field of the ceramic body, and when the grain size reaches the critical grain size, the polarization intensity will also change significantly, so preparing a ceramic body with a significant grain size effect is one of the means to optimize and improve the energy storage density. Generally, it is difficult to achieve the preparation of nanocrystalline ceramics through traditional solid-phase sintering, and the size effect of ceramics is often manifested in the submicron or even one or two hundred nanometers, so it is crucial to find a suitable preparation method. In addition, in an air environment, Ag2O and Nb2O5 cannot be well reacted at high temperature to obtain single-phase AN, so it is necessary to prepare high-quality AN ceramics in an oxygen-rich environment, which leads to high costs for preparing silver niobate ceramics with grain size effects, and the reaction process is unstable. In this regard, the existing market urgently needs a method that can stably and efficiently prepare silver niobate ceramics with grain size. Summary of the invention
[0004] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a silver niobate energy storage ceramic with high efficiency grain size effect. The ceramic material has a dense structure based on the microstructure, clear grains and grain boundaries, which gives the material an obvious grain size effect. On the basis of the original silver niobate energy storage ceramic, its energy storage performance is greatly improved. Compared with silver niobate energy storage ceramics without grain size effect, its energy storage performance is improved by up to 92%.
[0005] The second object of the present invention is to provide a method for preparing silver niobate energy storage ceramics with high-efficiency grain size effect. The method first prepares single-phase AN pre-fired powder by a solid phase reaction method, and then uses SPS sintering technology to obtain a dense ceramic body with obvious grain size effect; the method can also apply pressure in real time during sintering to obtain a higher density than the traditional solid phase method, and can greatly reduce the sintering temperature while ensuring high density, thereby obtaining a ceramic body with a dense structure and fine grains, successfully realizing the optimization and improvement of the energy storage density of AN ceramics.
[0006] Based on the SPS plasma sintering process, the rapid sintering of ceramic materials is achieved at a lower temperature.
[0007] Compared with the prior art, the present invention provides a method for preparing silver niobate energy storage ceramics with high efficiency grain size effect, wherein Ag2O and Nb2O5 are mixed evenly and then pre-sintered in oxygen to obtain pre-sintered powder; the pre-sintered powder is placed in a mold and subjected to SPS sintering to obtain dense ceramics, which are then subjected to decarburization treatment and electrode treatment to obtain;
[0008] The molar ratio of Ag2O to Nb2O5 is 1:0.8-1.2;
[0009] The temperature of the SPS sintering process is 700-1050° C., the pressure is 40-120 MPa, and the time is 3-7 minutes.
[0010] As a preferred solution, the mixing process of Ag2O and Nb2O5 is wet ball milling, the ball milling medium is anhydrous ethanol, and the grinding balls are ZrO2 grinding balls with a diameter of 2 to 8 mm.
[0011] As a preferred solution, during the ball milling mixing process, the mass ratio of powder, ball milling medium and grinding balls is 1:1-1.5:5-10, and the powder is ball milled to a particle size of ≤300 nm.
[0012] As a preferred solution, the ball milling mixing time is 24 to 48 hours, and the ball milling speed is 300 to 400 r / min.
[0013] As a preferred solution, the conditions for aerobic pre-burning are: temperature of 800-900°C, time of 3-6 hours, and oxygen flow rate of 0.2-0.8 L / min.
[0014] As a preferred solution, the pre-burned powder needs to be dried and sieved before being placed in the mold.
[0015] As a preferred solution, the drying conditions are: drying at 80-120° C. for 12-36 hours.
[0016] As a preferred solution, the mesh size of the sieving is 200-300 meshes.
[0017] As a preferred solution, the conditions of the SPS sintering process are: heating from room temperature to 750-950°C at 80-120°C / min, pressure of 50-90MPa, and time of 5-7min. Further preferably, the temperature of the SPS sintering process is 800-950°C, and most preferably, the temperature of the SPS sintering process is 930°C.
[0018] As a preferred solution, the decarburization process is: decarburization treatment is performed for 12 to 24 hours in an air atmosphere at a temperature of 760 to 940°C.
[0019] As a preferred solution, the electrode process is: brushing silver paste on the surface of the decarburized ceramic sheet, drying and sintering the electrode to obtain the electrode.
[0020] As a preferred solution, the electrode is sintered at a temperature of 500-600° C. for 10-30 minutes.
[0021] As a preferred solution, the diameter of the electrode is 2-4 mm, and the drying temperature is 760-940°C.
[0022] The present invention also provides a silver niobate energy storage ceramic with high efficiency grain size effect, which is prepared by any of the above methods.
[0023] Compared with the prior art, the beneficial technical effects of the present invention are:
[0024] 1) The silver niobate energy storage ceramic provided by the present invention has a dense structure based on the microstructure, clear grains and grain boundaries, which gives the material an obvious grain size effect. On the basis of the original silver niobate energy storage ceramic, its energy storage performance is greatly improved. Compared with the silver niobate energy storage ceramic without grain size effect, its energy storage performance is improved by up to 92%.
[0025] 2) The preparation method provided by the present invention first prepares single-phase AN pre-fired powder by a solid phase reaction method, and then uses SPS sintering technology to obtain a dense ceramic body with a significant grain size effect; this method can also apply pressure in real time during sintering to obtain a higher density than the traditional solid phase method, and can significantly reduce the sintering temperature while ensuring high density, thereby obtaining a ceramic body with a dense structure and fine grains, successfully realizing the optimization and improvement of the energy storage density of AN ceramics. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The ferroelectric hysteresis loop of the silver niobate ceramic prepared in Examples 1 to 4;
[0027] Figure 2 The surface morphology photos of the silver niobate ceramics prepared in Examples 1 to 4;
[0028] Figure 3 The X-ray diffraction patterns of the silver niobate ceramics prepared in Examples 1 to 4;
[0029] Figure 4 The dielectric temperature spectra of the silver niobate ceramics prepared in Examples 1 to 4 are shown. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0031] Example 1
[0032] Ag2O and Nb2O5 were used as raw materials and weighed according to the stoichiometric ratio. Then, anhydrous ethanol was used as the ball milling medium and the mixture was planetarily ball milled in a nylon ball mill filled with zirconium dioxide grinding balls for 24 hours at a speed of 300 rpm. After the powder was dried, it was placed in a corundum ark and calcined at 850°C for 6 hours in a tubular sintering furnace with a flowing O2 atmosphere. After it cooled, anhydrous ethanol was used as the ball milling medium to crush the calcined powder for a second time for 48 hours at a ball milling speed of 350 rpm to obtain the nanopowder (100-300 nm) required for the experiment. After obtaining the AN nanopowder, a certain amount of powder was weighed and placed in a high-strength graphite mold with a diameter of 20 mm, and then AN ceramics were prepared by SPS. The sintering temperature of SPS for preparing AN ceramics was 775°C, the applied pressure of the graphite mold was 90 MPa, the heating and cooling rate was 100°C / min, and the sintering time was 5 min. The decarburization time of AN ceramics in the muffle furnace is 24 h, the decarburization temperature is 760°C, and the obtained product is recorded as AN775 ceramics.
[0033] Example 2
[0034] According to the steps in Example 1, the nanopowder (100-300nm) required for the experiment was prepared, a certain amount of powder was weighed, and it was placed in a high-strength graphite mold with a diameter of 20mm, and then AN ceramics were prepared by SPS. The sintering temperature of AN ceramics prepared by SPS is 850℃, the applied pressure of the graphite mold is 50MPa, the heating and cooling rate is 100℃ / min, and the sintering time is 5min. The decarburization time of AN ceramics in the muffle furnace is 18h, the decarburization temperature is 830℃, and the obtained product is recorded as AN850 ceramics.
[0035] Example 3
[0036] According to the steps in Example 1, the nanopowder (100-300nm) required for the experiment was prepared, a certain amount of powder was weighed, and it was placed in a high-strength graphite mold with a diameter of 20mm, and then AN ceramics were prepared by SPS. The sintering temperature of AN ceramics prepared by SPS is 930℃, the applied pressure of the graphite mold is 50MPa, the heating and cooling rate is 100℃ / min, and the sintering time is 5min. The decarburization time of AN ceramics in the muffle furnace is 15h, the decarburization temperature is 900℃, and the obtained product is recorded as AN930 ceramics.
[0037] Example 4
[0038] According to the steps in Example 1, the nanopowder (100-300 nm) required for the experiment was prepared, a certain amount of powder was weighed, and it was placed in a high-strength graphite mold with a diameter of 20 mm, and then AN ceramics were prepared by SPS. The sintering temperature of AN ceramics prepared by SPS is 1040°C, the applied pressure of the graphite mold is 50 MPa, the heating and cooling rate is 100°C / min, and the sintering time is 5 min. The decarburization time of AN ceramics in the muffle furnace is 12 h, the decarburization temperature is 940°C, and the obtained product is recorded as AN1040 ceramics.
[0039] The energy storage characteristics of the AN antiferroelectric energy storage ceramics prepared in the above embodiment were tested, and the ferroelectric hysteresis loop was as follows: Figure 1 The specific performance indicators are shown in Table 1.
[0040] Table 1
[0041] sample <![CDATA[W rec (J / cm 3 )]]> η AN775 1.3 39.8 AN850 2.3 45.4 AN930 2.5 42.1 AN1040 2.0 40.2
[0042] Furthermore, the present invention also characterized the surface morphology of the samples obtained in Examples 1 to 4. The results are as follows: Figure 2 As shown, through Figure 2 It can be seen that the samples obtained in the present invention have a dense microstructure, and their grains and grain boundaries are clearly visible. The average grain storage of the samples obtained in Examples 1 to 4 gradually increases with the increase of sintering temperature, and their average grain sizes are 122.5±49.1nm, 226.8±106.2nm, 1.1±0.5μm and 2.7±1.0μm, respectively.
[0043] The present invention also carries out XRD characterization on the phase structure of the silver niobate ceramics prepared in Examples 1 to 4, and the results are as follows: Figure 3As shown, except for the sample obtained in Example 1 which has a trace amount of impurity AgNb3O8, the other three samples (AN850, AN930 and AN1040) all have pure phases. As the SPS sintering temperature increases, the diffraction peaks near 32°, 46° and 57° gradually separate, and the positions of the peaks also shift significantly, indicating that different grain sizes have a significant effect on the phase structure of AN ceramics. Then, the dielectric properties of the silver niobate ceramics prepared in Examples 1 to 4 were characterized, and the results are shown in Figure 2. Figure 4 As shown in Table 2, with the increase of the ceramic grain size, its phase transition temperature has changed significantly. The average grain size corresponding to the AN930 ceramic is the critical value for the phase transition to produce a significant grain size effect. For the AN850 sample with an average grain size smaller than the critical value, the phase transition temperature of the M phase transition and the M3→O phase transition moves to a lower direction. For the AN1040 sample with an average grain size larger than the critical value, the phase transition temperature of the M phase transition and the M3→O phase transition tends to be stable. The phase transition temperature of the AN775 sample is abnormal compared with the AN850 sample, which may be mainly caused by trace impurities and a large number of oxygen vacancies generated during low-temperature sintering. This conclusion is consistent with the energy storage characteristics test results obtained in Table 1, that is, the AN930 ceramic has the highest energy storage effect and its grain size effect is also the most obvious.
[0044] Table 2
[0045]
[0046]
Claims
1. A method for preparing silver niobate energy storage ceramics with high efficiency grain size effect, characterized in that: Ag2O and Nb2O5 are mixed evenly and then pre-sintered in oxygen to obtain pre-sintered powder; the pre-sintered powder is placed in a mold and sintered by SPS to obtain dense ceramics, which are then decarburized and electroded to obtain; The molar ratio of Ag2O to Nb2O5 is 1:0.8-1.2; The temperature of the SPS sintering process is 700-1050° C., the pressure is 40-120 MPa, and the time is 3-7 minutes.
2. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 1, characterized in that: The mixing process of Ag2O and Nb2O5 is wet ball milling mixing, the ball milling medium is anhydrous ethanol, and the grinding balls are ZrO2 grinding balls with a diameter of 2 to 8 mm.
3. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 2, characterized in that: During the ball milling mixing process, the mass ratio of powder, ball milling medium and grinding ball is 1:1-1.5:5-10, and the powder is ball milled to a particle size of ≤300nm; the ball milling mixing time is 24-48h, and the ball milling speed is 300-400r / min.
4. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 1, characterized in that: The conditions of the aerobic pre-burning are: temperature of 800-900° C., time of 3-6 hours, and oxygen flow rate of 0.2-0.8 L / min.
5. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 1, characterized in that: The pre-burned powder needs to be dried and sieved before being placed in the mold; the drying conditions are: drying at 80-120° C. for 12-36 hours; the mesh number of the sieve is 200-300 meshes.
6. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 1, characterized in that: The conditions of the SPS sintering process are: heating from room temperature to 750-950° C. at 80-120° C. / min, pressure of 50-90 MPa, and time of 5-7 min.
7. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 1, characterized in that: The decarburization process is as follows: decarburization is performed for 12 to 24 hours in an air atmosphere at a temperature of 760 to 940°C.
8. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 1, characterized in that: The electrode process is as follows: brushing silver paste on the surface of the decarbonized ceramic sheet, drying and sintering the electrode to obtain the electrode; the electrode sintering temperature is 500-600°C and the time is 10-30 minutes.
9. The method for preparing a silver niobate energy storage ceramic with high efficiency grain size effect according to claim 8, characterized in that: The diameter of the electrode is 2-4 mm, and the drying temperature is 760-940° C.
10. A silver niobate energy storage ceramic with high efficiency grain size effect, characterized in that: Prepared by the method described in any one of claims 1 to 9.
Citation Information
Patent Citations
NN-based energy storage ceramic block material with high energy storage density and energy storage efficiency and preparation method of NN-based energy storage ceramic block material
CN115376825A
Method for producing ceramic material based on bismuth-zinc-niobium oxides
RU2804938C1
Silver niobate ferroelectric materials
US2947698A
Piezoelectric ceramics
WO2004074209A1