Lightweight microporous sound insulation ceramic plate and preparation method thereof
By preparing lightweight microporous ceramic plates, using the combination of raw materials such as alumina, silicon carbide and boron nitride and additives such as adhesives, the problem of damage and poor sound insulation effect of ceramic plates under corrosive substances is solved, and the ceramic plates are realized Improved durability and sound insulation.
Patent Information
- Application Number
- CN202411151096.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
Existing ceramic plates are severely damaged when encountering corrosive substances, have short service life and poor sound insulation effect, making it difficult to prevent the spread of noise and affect users' daily life.
Using lightweight microporous soundproofing ceramic plate, after ball milling raw materials such as alumina, silicon carbide and boron nitride, adhesives, rheological agents, fire retardants, hardeners and antioxidants, dried, molded, fired and put them on. Prepare glaze and other steps to improve the bonding force, fire resistance and sound insulation of ceramic plates.
Ceramic plates have improved impact resistance, scratch resistance, wear resistance, fire resistance, moisture resistance and long service life. Soundproof coatings have excellent adhesion and aging resistance, which effectively improves the use effect and economic value of ceramic plates.
Smart Images

Figure CN118930274A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic plates, and in particular to a lightweight microporous sound-insulating ceramic plate and a preparation method thereof. Background Art
[0002] Ceramic panels made of zirconium oxide or aluminum oxide have strong weather resistance. Sunlight, rain (even acid rain), and moisture have no effect on the surface and substrate. The UV resistance and color stability fully meet the international grayscale level 4-5.
[0003] The anti-corrosion and sound insulation effects of ceramic plates are average. If they encounter corrosive substances, they will be damaged and the service life of the ceramic plates will be reduced. The sound insulation effect is poor and it is not convenient to prevent noise propagation, which affects the daily life of users. For this reason, we propose a lightweight microporous sound insulation ceramic plate and its preparation method. Summary of the invention
[0004] The purpose of the present invention is to solve the problems mentioned in the above background technology. The present invention provides a lightweight microporous sound insulation ceramic plate and a preparation method thereof.
[0005] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:
[0006] A lightweight microporous sound-insulating ceramic plate comprises a ceramic plate body, wherein the ceramic plate body comprises the following raw materials in parts by weight: 92-96 parts of matrix powder, 0.5-1 parts of adhesive, 0.5-1 parts of rheological agent, 0.5-1 parts of solvent raw materials, 0.5-1 parts of thickener, 0.5-1 parts of pigment, 0.5-1 parts of fire retardant, 0.5-1 parts of hardener and 0.5-1 parts of antioxidant additive.
[0007] Furthermore, the ceramic plate body includes the following raw materials by weight: 96 parts of base powder, 0.5 parts of adhesive, 0.5 parts of rheological agent, 0.5 parts of solvent raw materials, 0.5 parts of thickener, 0.5 parts of pigment, 0.5 parts of fire retardant, 0.5 parts of hardener and 0.5 parts of antioxidant additive.
[0008] Furthermore, the ceramic plate body includes the following raw materials by weight: 92 parts of base powder, 1 part of adhesive, 1 part of rheological agent, 1 part of solvent raw material, 1 part of thickener, 1 part of pigment, 1 part of fire retardant, 1 part of hardener and 1 part of antioxidant additive.
[0009] Furthermore, the ceramic plate body includes the following raw materials by weight: 94 parts of base powder, 0.75 parts of adhesive, 0.75 parts of rheological agent, 0.75 parts of solvent raw materials, 0.75 parts of thickener, 0.75 parts of pigment, 0.75 parts of fire retardant, 0.75 parts of hardener and 0.75 parts of antioxidant additive.
[0010] Furthermore, the matrix powder comprises the following raw materials in parts by weight: 20-30 parts of aluminum oxide, 35-40 parts of silicon carbide and 35-40 parts of boron nitride.
[0011] Furthermore, the matrix powder comprises the following raw materials in parts by weight: 20 parts of aluminum oxide, 40 parts of silicon carbide and 40 parts of boron nitride.
[0012] Furthermore, the matrix powder comprises the following raw materials in parts by weight: 25 parts of aluminum oxide, 37.5 parts of silicon carbide and 37.5 parts of boron nitride.
[0013] Furthermore, the matrix powder comprises the following raw materials in parts by weight: 30 parts of aluminum oxide, 35 parts of silicon carbide and 35 parts of boron nitride.
[0014] A method for preparing a lightweight microporous sound-insulating ceramic plate comprises the following steps:
[0015] S1. Prepare the blank, put aluminum oxide, silicon carbide and boron nitride into a ball mill according to the formula, and mix them evenly, so that the fineness of the mixture obtained by ball milling reaches 1% at 300 mesh;
[0016] S2, mixing raw materials, placing the ground and sieved blanks into a mixer, and before mixing, adding adhesives, rheological agents, solvent raw materials, thickeners, pigments, fire retardants, hardeners and antioxidant additives according to the formula weight;
[0017] S3, preliminary drying, placing the mixed raw materials in a dryer for heating and drying, and the drying time is 2 hours and the drying temperature is 75°C;
[0018] S4, preparing a green body, placing the raw materials after preliminary drying into a corresponding mold, and pressing it to form it;
[0019] S5, coating, coating the sound insulation coating evenly on the formed body;
[0020] S6, firing, placing the coated green body in a kiln for firing;
[0021] S7, glazing, glazing the fired ceramic plate.
[0022] Furthermore, the S6 is fired at a temperature of 1000° C.-1200° C., and the firing time is 12 hours.
[0023] The beneficial effects of the present invention are as follows:
[0024] The adhesive of the present invention enhances the internal bonding force of the ceramic plate; the thickener is used to increase the viscosity of the ceramic plate, making the ceramic plate easier to process and shape; the fire retardant is used to improve the fire resistance of the ceramic plate and reduce its combustion risk; the hardener is used to improve the hardness and wear resistance of the ceramic plate; the antioxidant is used to prevent the ceramic plate from oxidizing in a high temperature environment and extend its service life; the sound insulation paint is easy to apply, has excellent adhesion, excellent color retention and anti-aging properties, and has many functions such as mildew and algae resistance, alkali resistance, and ultraviolet radiation resistance, and can effectively improve the use effect and service life of the ceramic plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a work flow chart of the present invention. DETAILED DESCRIPTION
[0026] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0027] The present invention provides a lightweight microporous sound insulation ceramic plate, comprising a ceramic plate body, which comprises the following raw materials in parts by weight: 92-96 parts of matrix powder, 0.5-1 parts of adhesive, 0.5-1 parts of rheological agent, 0.5-1 parts of solvent raw materials, 0.5-1 parts of thickener, 0.5-1 parts of pigment, 0.5-1 parts of fire retardant, 0.5-1 parts of hardener and 0.5-1 parts of antioxidant additive, wherein the matrix powder comprises the following raw materials in parts by weight: 20-30 parts of aluminum oxide, 35-40 parts of silicon carbide and 35-40 parts of boron nitride.
[0028] Ceramic plates have the advantages of impact resistance, scratch resistance, wear resistance, fire resistance, moisture resistance, chemical corrosion resistance, etc. They have a long service life and high economic value. Adhesives are important materials for bonding ceramic powders together. Common ones include protein glue and polyvinyl alcohol. Their main function is to enhance the internal bonding force of ceramic plates. Rheological agents are used to adjust the fluidity of ceramic powders to make them easier to process and shape during the manufacturing process. Common ones include sodium polyacrylate and carboxymethyl cellulose. Solvents: Solvents are generally used to adjust the viscosity of ceramic powders and adhesives to make them more suitable for mold injection and molding. Thickeners: used to increase the viscosity of ceramic plates to make them easier to process and shape. Pigments: used to add color to ceramic plates to make them more beautiful. Fire retardants: used to improve the fire resistance of ceramic plates and reduce their risk of combustion. Hardeners: used to increase the hardness and wear resistance of ceramic plates. Antioxidants: used to prevent ceramic plates from oxidizing in high temperature environments and extend their service life.
[0029] Example 1
[0030] The ceramic plate body includes the following raw materials in parts by weight: 96 parts of base powder, 0.5 parts of adhesive, 0.5 parts of rheological agent, 0.5 parts of solvent raw materials, 0.5 parts of thickener, 0.5 parts of pigment, 0.5 parts of fire retardant, 0.5 parts of hardener and 0.5 parts of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 20 parts of aluminum oxide, 40 parts of silicon carbide and 40 parts of boron nitride.
[0031] Example 2
[0032] The ceramic plate body includes the following raw materials in parts by weight: 96 parts of base powder, 0.5 parts of adhesive, 0.5 parts of rheological agent, 0.5 parts of solvent raw material, 0.5 parts of thickener, 0.5 parts of pigment, 0.5 parts of fire retardant, 0.5 parts of hardener and 0.5 parts of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 25 parts of aluminum oxide, 37.5 parts of silicon carbide and 37.5 parts of boron nitride.
[0033] Example 3
[0034] The ceramic plate body includes the following raw materials in parts by weight: 96 parts of base powder, 0.5 parts of adhesive, 0.5 parts of rheological agent, 0.5 parts of solvent raw materials, 0.5 parts of thickener, 0.5 parts of pigment, 0.5 parts of fire retardant, 0.5 parts of hardener and 0.5 parts of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 30 parts of aluminum oxide, 35 parts of silicon carbide and 35 parts of boron nitride.
[0035] Example 4
[0036] The ceramic plate body includes the following raw materials in parts by weight: 92 parts of base powder, 1 part of adhesive, 1 part of rheological agent, 1 part of solvent raw material, 1 part of thickener, 1 part of pigment, 1 part of fire retardant, 1 part of hardener and 1 part of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 20 parts of aluminum oxide, 40 parts of silicon carbide and 40 parts of boron nitride.
[0037] Example 5
[0038] The ceramic plate body includes the following raw materials in parts by weight: 92 parts of base powder, 1 part of adhesive, 1 part of rheological agent, 1 part of solvent raw material, 1 part of thickener, 1 part of pigment, 1 part of fire retardant, 1 part of hardener and 1 part of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 25 parts of aluminum oxide, 37.5 parts of silicon carbide and 37.5 parts of boron nitride.
[0039] Example 6
[0040] The ceramic plate body includes the following raw materials in parts by weight: 92 parts of base powder, 1 part of adhesive, 1 part of rheological agent, 1 part of solvent raw material, 1 part of thickener, 1 part of pigment, 1 part of fire retardant, 1 part of hardener and 1 part of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 30 parts of aluminum oxide, 35 parts of silicon carbide and 35 parts of boron nitride.
[0041] Example 7
[0042] The ceramic plate body includes the following raw materials in parts by weight: 94 parts of base powder, 0.75 parts of adhesive, 0.75 parts of rheological agent, 0.75 parts of solvent raw materials, 0.75 parts of thickener, 0.75 parts of pigment, 0.75 parts of fire retardant, 0.75 parts of hardener and 0.75 parts of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 20 parts of aluminum oxide, 40 parts of silicon carbide and 40 parts of boron nitride.
[0043] Example 8
[0044] The ceramic plate body includes the following raw materials in parts by weight: 94 parts of base powder, 0.75 parts of adhesive, 0.75 parts of rheological agent, 0.75 parts of solvent raw material, 0.75 parts of thickener, 0.75 parts of pigment, 0.75 parts of fire retardant, 0.75 parts of hardener and 0.75 parts of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 25 parts of aluminum oxide, 37.5 parts of silicon carbide and 37.5 parts of boron nitride.
[0045] Example 9
[0046] The ceramic plate body includes the following raw materials in parts by weight: 94 parts of base powder, 0.75 parts of adhesive, 0.75 parts of rheological agent, 0.75 parts of solvent raw materials, 0.75 parts of thickener, 0.75 parts of pigment, 0.75 parts of fire retardant, 0.75 parts of hardener and 0.75 parts of antioxidant additive, among which the base powder includes the following raw materials in parts by weight: 30 parts of aluminum oxide, 35 parts of silicon carbide and 35 parts of boron nitride.
[0047] See also Figure 1 A method for preparing a lightweight microporous sound insulation ceramic plate comprises the following steps:
[0048] S1. Prepare the blank, put aluminum oxide, silicon carbide and boron nitride into a ball mill according to the formula, and mix them evenly so that the fineness of the mixture obtained by ball milling reaches 1% under 300 mesh; grind the blank to shorten the mixing time and improve work efficiency.
[0049] S2, raw material mixing, the blank after grinding and screening is placed in a mixer, and before mixing, adhesives, rheological agents, solvent raw materials, as well as thickeners, pigments, fire retardants, hardeners and antioxidant additives are added according to the formula weight.
[0050] S3, preliminary drying, placing the mixed raw materials in a dryer for heating and drying, and the drying time is 2 hours, and the drying temperature is 75°C; the raw materials can be condensed into blocks, and preliminary shaping can be achieved.
[0051] S4, preparing a green body, placing the raw materials after preliminary drying into a corresponding mold, and pressing it to form it; under the action of the mold and the press, the ceramic plate can be quickly formed.
[0052] S5. Paint, evenly apply the sound insulation paint on the formed body; the sound insulation paint is easy to apply, has excellent adhesion, excellent color retention and anti-aging, mildew and algae resistance, alkali resistance, anti-ultraviolet radiation and many other functions, which can effectively improve the use effect and service life of the ceramic board.
[0053] S6, firing, placing the coated body in a kiln for firing, the firing temperature is 1000°C-1200°C, and the firing time is 12 hours; firing can improve the hardness and wear resistance of the ceramic plate, improve the color and gloss of the ceramic plate, and ensure long-term use effect.
[0054] S7, glazing, glazing the fired ceramic plate; coating the fired blank with a layer of glassy glaze, which mainly plays a protective and decorative role.
[0055] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A lightweight microporous sound insulation ceramic plate, characterized in that: It includes a ceramic plate body, which includes the following raw materials by weight: 92-96 parts of base powder, 0.5-1 part of adhesive, 0.5-1 part of rheological agent, 0.5-1 part of solvent raw material, 0.5-1 part of thickener, 0.5-1 part of pigment, 0.5-1 part of fire retardant, 0.5-1 part of hardener and 0.5-1 part of antioxidant additive.
2. The lightweight microporous sound insulation ceramic plate according to claim 1, characterized in that: The ceramic plate body includes the following raw materials by weight: 96 parts of base powder, 0.5 parts of adhesive, 0.5 parts of rheological agent, 0.5 parts of solvent raw materials, 0.5 parts of thickener, 0.5 parts of pigment, 0.5 parts of fire retardant, 0.5 parts of hardener and 0.5 parts of antioxidant additive.
3. The lightweight microporous sound insulation ceramic board according to claim 1 is characterized in that: The ceramic plate body includes the following raw materials by weight: 92 parts of base powder, 1 part of adhesive, 1 part of rheological agent, 1 part of solvent raw material, 1 part of thickener, 1 part of pigment, 1 part of fire retardant, 1 part of hardener and 1 part of antioxidant additive.
4. The lightweight microporous sound insulation ceramic board according to claim 1, characterized in that: The ceramic plate body includes the following raw materials by weight: 94 parts of base powder, 0.75 parts of adhesive, 0.75 parts of rheological agent, 0.75 parts of solvent raw materials, 0.75 parts of thickener, 0.75 parts of pigment, 0.75 parts of fire retardant, 0.75 parts of hardener and 0.75 parts of antioxidant additive.
5. The lightweight microporous sound insulation ceramic plate according to claim 1, characterized in that: The matrix powder comprises the following raw materials in parts by weight: 20-30 parts of aluminum oxide, 35-40 parts of silicon carbide and 35-40 parts of boron nitride.
6. The lightweight microporous sound insulation ceramic plate according to claim 5, characterized in that: The matrix powder comprises the following raw materials in parts by weight: 20 parts of aluminum oxide, 40 parts of silicon carbide and 40 parts of boron nitride.
7. The lightweight microporous sound insulation ceramic plate according to claim 5, characterized in that: The matrix powder comprises the following raw materials in parts by weight: 25 parts of aluminum oxide, 37.5 parts of silicon carbide and 37.5 parts of boron nitride.
8. The lightweight microporous sound insulation ceramic plate according to claim 5, characterized in that: The matrix powder comprises the following raw materials in parts by weight: 30 parts of aluminum oxide, 35 parts of silicon carbide and 35 parts of boron nitride.
9. A method for preparing a lightweight microporous sound insulation ceramic plate, characterized in that: The steps include: S1. Prepare the blank, put aluminum oxide, silicon carbide and boron nitride into a ball mill according to the formula, and mix them evenly, so that the fineness of the mixture obtained by ball milling reaches 1% at 300 mesh; S2, mixing raw materials, placing the ground and sieved blanks into a mixer, and before mixing, adding adhesives, rheological agents, solvent raw materials, thickeners, pigments, fire retardants, hardeners and antioxidant additives according to the formula weight; S3, preliminary drying, placing the mixed raw materials in a dryer for heating and drying, and the drying time is 2 hours and the drying temperature is 75°C; S4, preparing a green body, placing the raw materials after preliminary drying into a corresponding mold, and pressing it to form it; S5, coating, coating the sound insulation coating evenly on the formed body; S6, firing, placing the coated green body in a kiln for firing; S7, glazing, glazing the fired ceramic plate.
10. The method for preparing a lightweight microporous sound insulation ceramic board according to claim 9, characterized in that: The S6 is fired at a temperature of 1000° C.-1200° C. and for a time of 12 hours.
Citation Information
Patent Citations
Microporous ceramic and preparation method thereof
CN107200566A
Inner wall heat-preservation flame-retardant diatom ooze and preparation method
CN107778929A
Environment-friendly sound insulation and noise reduction coating
CN107868562A
Sound absorption ceramic and preparation method thereof